A blended fabric and anti-pilling technology, applied in the field of cotton-linen blended fabric and its anti-pilling smooth finishing, multi-functional cotton-linen blended fabric finishing, can solve problems for consumers and manufacturers, affect product use value and economy Value and other issues, to achieve the effect of reducing the pilling rate, increasing economic benefits and practicability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] In the first step, cotton and linen are blended at 40%: 60%.
[0020] Step 2, singeing, burner: one front and one reverse, the speed of the machine is 110m / min, and the singeing effect reaches level 5.
[0021] The third step is to process the bleached cotton and linen blended fabrics. First, prepare a finishing solution, and soak the cotton and linen blended fabrics in the finishing solution. The immersion temperature is 60°C, and the immersion time is 65 minutes. The rate is 100%, pre-bake at 90°C for 3 minutes, and then bake at 150°C for 3 minutes.
[0022] In the third step, the finishing liquid includes 21 parts of polyurethane resin, 12 parts of magnesium chloride and 65 parts of purified water in parts by weight.
[0023] In the fourth step, soft finishing, dipping temperature in softener is 50°C, dipping time is 45min, one dipping and one padding, the scrapping rate is 85%, bake at 90°C for 2min, rinse with 35°C water for 3 times, bake at 60°C Dry for 6 minute...
Embodiment 2
[0025] Step 1: Cotton and linen are blended at 35%:65%.
[0026] Step 2: singeing, burner: one front and one reverse, the speed of the machine is 90m / min, and the singeing effect reaches grade 3.
[0027] Step 3: Finish the bleached cotton and linen blended fabric, first prepare the finishing solution, and soak the cotton and linen blended fabric in the finishing solution, the immersion temperature is 55°C, the immersion time is 55min, two dipping and two rolling, The rate is 95%, pre-bake at 80-95°C for 2 minutes, and then bake at 155°C for 2 minutes.
[0028] In the third step, the finishing liquid includes 21 parts of polyurethane resin, 15 parts of magnesium chloride and 54 parts of purified water in parts by weight.
[0029] Step 4: Soft finishing, dipping in softener at 45°C, dipping time for 45min, one dipping and one padding, 80% scrap rate, baking at 100°C for 3min, rinsing with 35°C water for 3 times, drying at 65°C 5min.
Embodiment 3
[0031] Step 1: Cotton and linen are blended at 30%:70%.
[0032] Step 2: singeing, burner: one positive and one reversed, the speed of the vehicle is 100m / min, and the singeing effect reaches level 4.
[0033] Step 3: Finish the bleached cotton and linen blended fabric, first prepare the finishing solution, and soak the cotton and linen blended fabric in the finishing solution, the immersion temperature is 55°C, the immersion time is 65min, two dipping and two rolling, The rate is 105%, prebaked at 90°C for 2 minutes, and then baked at 145°C for 3 minutes.
[0034] In the third step, the finishing liquid includes 18 parts of polyurethane resin, 16 parts of magnesium chloride and 60 parts of purified water in parts by weight.
[0035] Step 4: Soft finishing, immerse in the softener at a temperature of 50°C, immerse in a time of 45min, one dip and one rolling, the excess rate is 90%, bake at 100°C for 3min, rinse twice with water at 40°C, and dry at 60°C 5min.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com