Embodiment 1
[0041] This embodiment provides a kind of processing method of spandex super soft velvet, through the steps:
[0042] S1: Use 100D / 36F spandex filament as the base layer and 75D / 144F spandex smooth filament as the surface layer to make gray cloth;
[0043] S2: Arrange the blank on the setting machine, the setting temperature is 205°C, and the fleece travel speed is controlled at 30m / min;
[0044] S3: Using a napping machine to roughen the surface of the gray cloth;
[0045] S4: Ironing the fabric made of S3 on a single-roller ironing machine, the temperature of the hot roller is 200°C;
[0046] S5: Use a shearing machine to subtract long hair from the cloth made by S4;
[0047] S6:
[0048] a. Dyeing the cloth made of S5 in cylinder, the amount of disperse dye is 4% of the weight of flannelette, and the duration is 1 hour;
[0049] b. Out of cylinder;
[0050] c. Reduction cleaning, using water at 175°C to remove floating colors;
[0051] S7: Dry the fabric made of S6 in...
Embodiment 2
[0062] This embodiment provides a kind of processing method of spandex super soft velvet, through the steps:
[0063] S1: Use 100D / 36F spandex filament as the base layer and 75D / 144F spandex smooth filament as the surface layer to make gray fabric;
[0064] S2: Arrange the blanks on the setting machine, the setting temperature is 205°C, and the gray cloth travel speed is controlled at 36m / min;
[0065] S3: Using a napping machine to roughen the surface of the gray cloth;
[0066] S4: Ironing the fabric made of S3 on a single-roller ironing machine, the temperature of the hot roller is 210°C;
[0067] S5: Use a shearing machine to subtract long hair from the cloth made by S4;
[0068] S6:
[0069] a. Dyeing the cloth made of S5 into a cylinder, using disperse dyes in an amount of 7% of the flannelette weight, and the duration is 1 hour;
[0070] b. Out of cylinder;
[0071] c. Reduction cleaning, using water at 180°C (dye is easy to sublime above 180°C) to remove floating ...