A technology for emulsified asphalt and emulsification equipment, which is used in building components, building insulation materials, buildings, etc., can solve the problems of poor later service performance, slow early strength formation, poor construction and workability of cold recycled mixture, etc. The effect of bonding, reducing reflection cracks, and eliminating road surface diseases
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0025] (1) Heat the base asphalt to 135-140°C;
[0026] (2) Mix emulsifier SGT-1901, emulsifier SGT-1904, and water at a weight ratio of 2.0:0.58:100, then add hydrochloric acid to adjust the pH value to 1.9, prepare soap liquid, and heat the soap liquid to 35-40°C;
[0027] (3) Transport the soap liquid and matrix asphalt into the colloid mill respectively, wherein the weight ratio of matrix asphalt and soap liquid is 62:38. In order to prevent sundries from entering the colloid mill, a filter device is installed at the inlet of the colloid mill; After grinding and dispersing evenly, emulsified asphalt is obtained, and when the emulsified asphalt is cooled to 60-70°C, it is transported to a storage tank for storage.
Embodiment 2
[0029] (1) Heat the base asphalt to 135-140°C;
[0030] (2) Mix emulsifier SGT-1901, emulsifier SGT-1904, and water at a weight ratio of 2.2:0.38:100, then add hydrochloric acid to adjust the pH value to 2.1, prepare soap liquid, and heat the soap liquid to 35-40°C;
[0031] (3) Transport the soap liquid and matrix asphalt into the colloid mill respectively, wherein the weight ratio of matrix asphalt and soap liquid is 62:38. In order to prevent sundries from entering the colloid mill, a filter device is installed at the inlet of the colloid mill; After grinding and dispersing evenly, emulsified asphalt is obtained, and when the emulsified asphalt is cooled to 60-70°C, it is transported to a storage tank for storage.
Embodiment 3
[0033] (1) Heat the base asphalt to 135-140°C;
[0034] (2) Mix emulsifier SGT-1901, emulsifier SGT-1904, and water at a weight ratio of 1.8:0.78:100, then add hydrochloric acid to adjust the pH value to 1.7, prepare soap liquid, and heat the soap liquid to 35-40°C;
[0035] (3) Transport the soap liquid and matrix asphalt into the colloid mill respectively, wherein the weight ratio of matrix asphalt and soap liquid is 62:38. In order to prevent sundries from entering the colloid mill, a filter device is installed at the inlet of the colloid mill; After grinding and dispersing evenly, emulsified asphalt is obtained, and when the emulsified asphalt is cooled to 60-70°C, it is transported to a storage tank for storage.