Sludge solidification treatment framework construction method
A technology of sludge solidification and sludge, which is applied in the direction of sludge treatment, water/sludge/sewage treatment, solid waste management, etc., can solve the problems of occupying farmland or fishing ponds, polluting the environment of sludge dumping points, etc., and achieve reduction Environmental issues, treatment cost reduction, cost reduction effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0009] Each component of the present invention is mixed uniformly by following percentage by weight:
[0010] Sludge 63.5%
[0011] Cement 15.0%
[0012] Silt 21.5%
[0013] According to this ratio, 236.2kg of solidified material and 338.6kg of sludge are added to each ton of sludge, and the unconfined compressive strength of the solidified sludge can reach 50kPa in 7 days, and the water permeability coefficient of the solidified sludge is less than 10 -7 cm / s,
[0014] It can meet the needs of sludge for landfill disposal or as landfill covering soil. Compared with the method of not using skeleton construction, it can save nearly 10 times the cost to achieve the same curing effect.
Embodiment 2
[0016] Each component of the present invention is mixed uniformly by following percentage by weight:
[0017] Sludge 55.1%
[0018] Cement 13.1%
[0019] Fly Ash 2.3%
[0020] Silt 29.5%
[0021] Using this ratio, add 279.5kg of solidified materials (cement and fly ash) and 535.4kg of sludge to each ton of sludge, and the unconfined compressive strength of the solidified sludge can reach 100kPa within 7 days. It can meet the requirements of filling soil in general engineering, and can save nearly 12 times the cost to achieve the same curing effect compared with the method of not using skeleton construction.
Embodiment 3
[0023] Each component of the present invention is mixed uniformly by following percentage by weight:
[0024] Sludge 57.5%
[0025] Cement 11.1%
[0026] Gypsum 2.7%
[0027] Fly Ash 2.2%
[0028] Silt 26.5%
[0029] Using this ratio, adding 278.3kg of solidified materials (cement, fly ash and gypsum) and 460.8kg of sludge to each ton of sludge, the unconfined compressive strength of the solidified sludge can reach 85kPa within 7 days. It can meet the requirements of filling soil in general engineering, and can save nearly 14 times the cost to achieve the same curing effect compared with the method of not using skeleton construction.
[0030] Explanation of the principle of skeleton construction: Since the main solid components in the sludge are mainly organic matter and biological residues, while the inorganic solid particle components are very small, the strength formed after solidi...
PUM
Property | Measurement | Unit |
---|---|---|
Unconfined compressive strength | aaaaa | aaaaa |
Water permeability coefficient | aaaaa | aaaaa |
Unconfined compressive strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com