Cotton-real silk XLA intertexture and producing method thereof
A production method and interwoven fabric technology, applied in the direction of fabric, textile, textile and papermaking, etc., can solve the problems affecting the beauty and wearability of cotton fabrics, poor elasticity, uncomfortable wearing and so on
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment Construction
[0017] 1. Material selection:
[0018] Cotton (100 / 2) is used in the warp direction; silk (22D / 3) and XLA (50 / 42D) doubling yarns are used in the weft direction.
[0019] 2. Silk bobbin yarn winding, degumming, bobbin dyeing;
[0020] 1. Silk bobbin winding
[0021] 2. Degumming, pretreatment, dyeing:
[0022] Degumming pre-treatment one-bath process:
[0023] Auxiliary:
[0024] Soda ash: 0.5g / L~1.5g / L
[0025] Refining agent C-NEC: 1.5g / L~2g / L
[0026] Chelating agent M-PP: 1.5g / L~2g / L
[0027] h 2 o 2 Or reducing bleach Blankit IN: 2~4g / L
[0028] Process conditions:
[0029] Control the PH value at 9.5-10
[0030] Bath ratio: 1:20
[0031] Run at 95 degrees x 60 minutes
[0032] Followed by hot water washing, water washing, pickling for neutralization.
[0033] Silk Dyeing:
[0034] The pH value before dyeing is controlled at 6.5
[0035] Dyeing process:
[0036] Bath ratio: 1:20
[0037] DyStar RGB dye: the dosage is determined according to different col...
PUM

Abstract
Description
Claims
Application Information

- R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com