Wear-resisting farm machinery parts and heat treatment process thereof
A technology of accessories and agricultural machinery, which is applied in the field of heat treatment technology, can solve the problems of low service life, easy fracture, poor toughness, etc., and achieve the effect of reducing quenching stress and brittleness, high hardness and wear resistance, and increasing wear resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] A formula of white cast iron for wear-resistant agricultural machinery accessories is:
[0018] Fe: 67.5%, C: 3.1%; Si: 0.7%; Cr: 23.0%; Mn: 0.9%; Ni: 4.8%.
[0019] Its heat treatment process is:
[0020] (1) Pour the molten metal liquid into the sand mold, make it cast into castings, and set aside;
[0021] (2) Put the above-mentioned castings into a box-type resistance furnace for quenching treatment, the temperature is controlled at 920±10°C, and the holding time is 60 minutes;
[0022] (3) Air cooling the casting after quenching to room temperature;
[0023] (4) Place the air-cooled casting in a box-type resistance furnace for tempering treatment, the temperature is controlled at 230±10°C, and the holding time is 120 minutes;
[0024] (5) Air-cool the tempered casting to room temperature.
Embodiment 2
[0026] A formula of white cast iron for wear-resistant agricultural machinery accessories is:
[0027] Fe: 66.2%, C: 3.2%; Si: 0.8%; Cr: 24.5%; Mn: 0.8%; Ni: 4.5%.
[0028] Its heat treatment process is:
[0029] (1) Pour the molten metal liquid into the sand mold, make it cast into castings, and set aside;
[0030] (2) Put the above-mentioned castings into a box-type resistance furnace for quenching treatment, the temperature is controlled at 920±10°C, and the holding time is 60 minutes;
[0031] (3) Air cooling the casting after quenching to room temperature;
[0032] (4) Place the air-cooled casting in a box-type resistance furnace for tempering treatment, the temperature is controlled at 230±10°C, and the holding time is 120 minutes;
[0033] (5) Air-cool the tempered casting to room temperature.
Embodiment 3
[0035] A formula of gray cast iron for wear-resistant agricultural machinery accessories is:
[0036] Fe: 67.3%, C: 3.3%; Si: 0.9%; Cr: 23.0%; Mn: 1.0%; Ni: 4.5%.
[0037] Its heat treatment process is:
[0038] (1) Pour the molten metal liquid into the mold, make it cast into castings, and set aside;
[0039] (2) Put the above-mentioned castings into a box-type resistance furnace for quenching treatment, the temperature is controlled at 920±10°C, and the holding time is 60 minutes;
[0040] (3) Air cooling the casting after quenching to room temperature;
[0041] (4) Place the air-cooled casting in a box-type resistance furnace for tempering treatment, the temperature is controlled at 230±10°C, and the holding time is 120 minutes;
[0042] (5) Air-cool the tempered casting to room temperature.
PUM

Abstract
Description
Claims
Application Information

- R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com