Embodiment 1
[0015] Embodiment 1: Utilize 100S / 2 flax / cotton blended yarn to process the specific process steps of high-count flax / cotton blended knitted fabric as follows:
[0016] (1), add low foam penetration scouring agent DLF 0.5g / L, demineralizing agent EMG 1g / L in water to form a treatment solution, then put the flax / cotton blended yarn into the dyeing vat, control the flax / cotton blended yarn and The weight ratio of the treatment solution is 1:10, and it is treated at a temperature of 60° C. for 20 minutes;
[0017] (2), flax / cotton blended yarn was boiled at a high temperature of 100°C for 10 minutes;
[0018] (3), add softener AWG 2g / L in water to form a softener solution, then put the flax / cotton blended yarn boiled at high temperature into a high-temperature and high-pressure dyeing machine, and control the weight of the flax blended yarn and softener solution The ratio is 1:8, and it is treated at a temperature of 45°C for 20 minutes;
[0019] (4), feed the treated high-qual...
Embodiment 2
[0029] Embodiment two: utilize 80S / 2 flax / cotton blended yarn to process the specific technological steps of high-count flax / cotton blended knitted fabric as follows:
[0030] (1), add low-foam penetration scouring agent DLF 0.8g / L, demineralizer EMG 2g / L in water to form a treatment solution, then put flax / cotton blended yarn into the dyeing vat, control flax / cotton blended yarn and The weight ratio of the treatment solution is 1:8, and it is treated at a temperature of 70° C. for 25 minutes;
[0031] (2), flax / cotton blended yarn was boiled at a high temperature of 120°C for 15 minutes;
[0032] (3) Add softener AWG 1g / L to water to form a softener solution, then put the flax / cotton blended yarn boiled at high temperature into a high-temperature and high-pressure dyeing machine to control the weight of the flax blended yarn and softener solution The ratio is 1:7, and it is treated at a temperature of 50°C for 25 minutes;
[0033] (4), feed the treated high-quality flax / cot...
Embodiment 3
[0043] Embodiment Three: The specific process steps of processing high-count flax / cotton blended knitted fabrics with 80S / 1×2 flax / cotton blended yarn are:
[0044](1) Add 0.6g / L low-foaming penetrating scouring agent DLF and 1.5g / L demineralizer EMG to water to form a treatment solution, then put the flax / cotton blended yarn into the dyeing vat to control the flax / cotton blended yarn The weight ratio to the treatment solution is 1:9, and it is treated at a temperature of 50°C for 15 minutes;
[0045] (2), flax / cotton blended yarn was boiled at a high temperature of 90°C for 8 minutes;
[0046] (3), add softening agent AWG 1.5g / L in water to form softening agent solution, then put the flax / cotton blended yarn after high-temperature boiling into the high-temperature and high-pressure dyeing machine, control the balance of flax blended yarn and softening agent solution The weight ratio is 1:10, and treated at a temperature of 40° C. for 15 minutes;
[0047] (4), feed the treat...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com