Adhesive for artificial board and preparation method of adhesive

A technology for adhesives and wood-based panels, applied in the preparation of adhesives, animal glue or gelatin, adhesive types, etc., can solve the problems of reduced product bonding strength, increased product cost, and reduced production efficiency, so as to solve formaldehyde pollution and meet Water resistance requirements, the effect of comprehensive utilization of resources

Inactive Publication Date: 2015-01-21
BEIJING FORESTRY UNIVERSITY
View PDF3 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

For example: 1) Although the use of a low molar ratio modified urea-formaldehyde resin adhesive can effectively reduce the formaldehyde emission of wood-based panel products, the bonding strength of the product is often reduced, which cannot meet the requirements of use; and the curing time is prolonged and the production efficiency is reduced; 2) The use of other environmentally friendly adhesives, such as isocyanate adhesives, has led to a substantial increase in the production cost of wood-based panels, which is difficult for enterprises and users to accept; the wood-based panels prepared with ordinary protein adhesives have low bonding strength, and the wood-based panels are easy to open; 3) In artificial Adding formaldehyde scavenger to the urea-formaldehyde resin adhesive for boards can effectively reduce the release of free formaldehyde from wood-based panels, but it often reduces the bonding strength of wood-based panels; at the same time, the price of general formaldehyde scavenger is often much higher than that of urea-formaldehyde resin adhesives. Just improved product cost, reduced product competitiveness; 4) carry out post-processing to wood-based panel, disclose a kind of adopting ammonia gas vacuum method to prepare E1 / EO level environment-friendly type wood-based panel in the invention patent application of CN1526528 as publication number Manufacturing process; the utility model patent with publication number CN2394770 discloses a treatment device for reducing formaldehyde emission from wood-based panels. These post-processing methods not only make the manufacturing process of wood-based panels complicated, but also require huge investment in post-processing equipment and significant production costs. improve
In summary, although the above measures can effectively reduce the release of free formaldehyde from wood-based panels, they cannot completely solve the problem of formaldehyde release, or cannot be popularized due to reasons such as high production costs.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Adhesive for artificial board and preparation method of adhesive
  • Adhesive for artificial board and preparation method of adhesive
  • Adhesive for artificial board and preparation method of adhesive

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0026] The preparation of embodiment 1 adhesive

[0027] 1) Prepare materials according to the following weight ratio:

[0028]

[0029] Among them, the complexing agent is a powder prepared by the School of Materials Science and Technology of Beijing Forestry University, including zinc chloride: 0.8 parts, copper sulfate: 0.5 parts, zirconium carbonate: 0.5 parts, which are ground and mixed evenly; the reinforcing agent is 80 mesh powder of EVA with 20% vinyl acetate content and a melt index of 20.

[0030] 2) Add all the demineralized water, sodium carbonate and soy protein powder into the reaction kettle equipped with agitator, thermometer and condensing device, and stir evenly.

[0031] 3) Heat to 45-47°C and keep warm for 3 hours.

[0032] 4) The temperature of the reactant was lowered to 30°C to obtain a uniform soy protein mucus.

[0033] 5) Add complexing agent and enhancer to the obtained soy protein mucilage, mix well to make soy protein adhesive. The performa...

Embodiment 2

[0034] The preparation of embodiment 2 adhesive

[0035] 1) Prepare materials according to the following weight ratio:

[0036]

[0037] Among them, the complexing agent is a powder prepared by the School of Materials Science and Technology of Beijing Forestry University, including 1.2 parts of zinc chloride, 1.5 parts of copper sulfate, and 1.5 parts of zirconium carbonate, which are ground and mixed evenly; the reinforcing agent is vinyl acetate. A 100-mesh powder of EVA with a content of 25% and a melt index of 60.

[0038] 2) Add all the demineralized water, sodium carbonate, defatted soybean meal powder into the reaction kettle equipped with agitator, thermometer and condensing device, and stir evenly;

[0039] 3) Heat to 40-42°C and react for 6 hours;

[0040] 4) The temperature of the reactant was lowered to 30°C to obtain a uniform soy protein mucus.

[0041] 5) Add complexing agent and enhancer to the obtained soy protein mucilage, mix well to make soy protein a...

Embodiment 3

[0042] The preparation of embodiment 3 adhesive

[0043] 1) Prepare materials according to the following weight ratio:

[0044]

[0045] Among them, the complexing agent is a powder prepared by the School of Materials Science and Technology, Beijing Forestry University, including the following components in weight proportions: 0.8 parts of zinc chloride, 1.5 parts of copper sulfate, and 1 part of zirconium carbonate, which are ground evenly and mixed Uniform; the reinforcing agent is a 60-mesh powder of EVA with a vinyl acetate content of 40% and a melt index of 100.

[0046] 2) Add all the demineralized water, sodium carbonate and soy protein powder into the reaction kettle equipped with agitator, thermometer and condensing device, and stir evenly.

[0047] 3) Heat to 68-70°C and react for 5 hours.

[0048] 4) The temperature of the reactant was lowered to 30°C to obtain a uniform soy protein mucus.

[0049] 5) Add complexing agent and enhancer to the obtained soy prote...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention relates to an adhesive for an artificial board and a preparation method of the adhesive. The adhesive consists of the following raw materials: a dispersing medium, defatted protein powder, sodium carbonate, a complexing agent and a reinforcing agent, wherein the complexing agent is composed of zinc chloride, copper sulfate and zirconium carbonate; and the reinforcing agent is ethylene-vinyl acetate copolymer (EVA) powder. According to the adhesive, the problem that the common soybean protein adhesive is poor in water resistance is solved, and the water resistance demand of the adhesive for the artificial board is met; and the adhesive is lower in curing temperature, faster in curing speed, easier in application and high in binding strength, and the industrial production is easy to realize.

Description

technical field [0001] The invention relates to an adhesive, in particular to an adhesive for wood-based panels and a preparation method thereof. Background technique [0002] With the rapid development of construction, decoration, packaging and other industries, the output of wood-based panels in my country has increased rapidly. In 2010, the total output of my country's wood-based panels was 153.6 million cubic meters, accounting for about 50% of the world's weight, including 71.3966 million cubic meters of plywood and 16.5228 million cubic meters of blockboard. The total output of wood-based panels, plywood, furniture, and wood flooring has ranked first in the world for many years in a row. [0003] The adhesives commonly used in the production of wood-based panels are formaldehyde-based synthetic resins, mainly urea-formaldehyde resins and their modified products. Although after years of hard work, the production level of wood-based panel adhesives in my country has be...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Patents(China)
IPC IPC(8): C09J189/00C09J11/04C09J11/08
Inventor 周文瑞张纪芝李建章张世锋高强
Owner BEIJING FORESTRY UNIVERSITY
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products