Poplar modifying process
A poplar, modified technology, applied in the direction of wood processing equipment, wood treatment, manufacturing tools, etc., can solve the problems of small one-time processing capacity and high equipment requirements, and achieve the effect of super-large-scale production, simple equipment and cost reduction.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] Poplar modified technique of the present invention comprises the following steps,
[0024] The first step is to test the material, and it is detected that the pH of the pretreated poplar is 5.5;
[0025] The second step is to peel and saw the poplar logs;
[0026] The third step, cooking: put 140 cubic meters of wood into a pool with 18.9 kg of sodium hydroxide solid particles, a water temperature of 40°C, and a water storage capacity of 126 tons, and cook for 15 days; the water is heated through a steam pipeline Constant temperature;
[0027] The fourth step is to drain the water in the pool first, then fill it with clear water at 5°C, and soak the poplar in clear water for two days;
[0028] The fifth step is to salvage the poplar and move it into the drying kiln;
[0029] The sixth step, drying: after the wood is put into the kiln, increase the temperature in the kiln to 20°C, keep it for one day, then increase it by 10°C every day, when it reaches 80°C, the tempe...
Embodiment 2
[0034] Poplar modified technique of the present invention comprises the following steps,
[0035] The first step is to test the material, and it is detected that the pH of the pretreated poplar is 7.8;
[0036] The second step is to peel and saw the poplar logs;
[0037] The third step, cooking: put 140 cubic meters of wood into a pool with a water temperature of 50°C and a water storage capacity of 155 tons, wherein the pool is added with 62 kg of hydrochloric acid solution with a mass fraction of 25%, and cook for 15 days;
[0038] The fourth step is to drain the water in the pool first, then fill it with clean water at 20°C, and soak the poplar in the clean water for two days;
[0039] The fifth step is to salvage the poplar and move it into the drying kiln;
[0040] The sixth step, drying: after the wood is put into the kiln, increase the temperature in the kiln to 20°C, keep it for one day, then increase it by 10°C every day, when it reaches 80°C, the temperature will n...
Embodiment 3
[0045] Poplar modified technique of the present invention comprises the following steps,
[0046] The first step is to test the material, and it is detected that the pH of the pretreated poplar is 5.5;
[0047] The second step is to peel and saw the poplar logs;
[0048] The third step, cooking: put 140 cubic meters of wood into a pool with 21 kg of sodium hydroxide solid particles, a water temperature of 45°C, and a water storage capacity of 140 tons, and cook for 15 days; the water is heated through a steam pipeline Constant temperature;
[0049] The fourth step is to drain the water in the pool first, then fill it with clean water at 10°C, and soak the poplar in the clean water for two days;
[0050] The fifth step is to salvage the poplar and move it into the drying kiln;
[0051] The sixth step, drying: After the wood is put into the kiln, increase the temperature in the kiln to 20°C, keep it for one day, then increase it by 10°C every day, when it reaches 80°C, the te...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com