Manufacturing method of heel lift
A manufacturing method, the technology of the skin, applied in applications, soles, clothing, etc., can solve problems such as embarrassment, loud noise, and inconvenience to others, and achieve the effect of comfortable wearing, good elasticity, and protection of the cervical spine and spine
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0017] Take making 100 kilograms of sky skin sheets as an example, the formula of the present embodiment is as follows:
[0018]
[0019] The process flow is as follows:
[0020] First put 45 kg of artificial rubber into a heating and stirring tank, heat it to 50°C, and keep it warm for 10 minutes. In the kettle, knead and stir well for 20 minutes until it is uniform; take out the fully synthesized material, add 2 kg of sulfur through an open mill, roll it into pieces, and cut it into shape; After the material is combined, put it into the heated mold, heat it to 155°C, keep it warm for 8 minutes, then take out the high-temperature mold, and cool it down to 40°C through water cooling.
Embodiment 2
[0022] Take making 100 kilograms of sky skin sheets as an example, the formula of the present embodiment is as follows:
[0023]
[0024] The process flow is as follows:
[0025] First put 75 kg of artificial rubber into a heating and stirring tank, heat it to 50°C, and keep it warm for 10 minutes. After the artificial rubber is fully softened, add 10 kg of granular polyvinyl chloride raw materials and 14 kg of white carbon black of 500 mesh In the kettle, knead and stir well for 20 minutes until it is uniform; take out the fully synthesized material, add 1 kg of sulfur through an open mill, roll it into pieces, and cut it into shape; After the material is combined, put it into the heated mold, heat it to 155°C, keep it warm for 8 minutes, then take out the high-temperature mold, and cool it down to 40°C through water cooling.
Embodiment 3
[0027] Take making 100 kilograms of sky skin sheets as an example, the formula of the present embodiment is as follows:
[0028]
[0029] The process flow is as follows:
[0030] First put 60 kg of artificial rubber into a heating and stirring tank, heat it to 50°C, and keep it warm for 10 minutes. After the artificial rubber is fully softened, add 15 kg of granular polyvinyl chloride raw materials and 22 kg of white carbon black of 500 mesh In the kettle, knead and stir well for 20 minutes until it is uniform; take out the fully synthesized materials, add 3 kg of sulfur through an open mill, roll them into pieces, and cut them into shapes; After the material is combined, put it into the heated mold, heat it to 155°C, keep it warm for 8 minutes, then take out the high-temperature mold, and cool it down to 40°C through water cooling.