Anti-shrinkage anti-pilling wool fabric finishing agent and preparation method thereof
An anti-shrinkage and finishing agent technology, applied in fiber processing, textiles and papermaking, etc., can solve problems such as easy pilling, felting reaction, shrinkage, etc., achieve high anti-pilling level and improve quality
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032] (1) Pour 9 parts of sodium tripolyphosphate, 8 parts of coumarin gum, 3 parts of polyethylene glycol, 11 parts of hydroxyethyl methacrylate, and 7 parts of allyl glycidyl ether into the container by weight, Stir for 5 minutes at a rotational speed of 120r / min, and it will be material A after stirring evenly;
[0033] (2) Take 9 parts of N-oleoyl-N-methyl taurate sodium, 3 parts of n-butanol, and 350 parts of water by weight, and mix the ingredients of step (2) in the container evenly, and it is B material ;
[0034] (3) Put the material A that has been stirred evenly in step (1) into material B, and then stir for 30 minutes at a speed of 120r / min, and then use a shearer to shear the mixed solution evenly. The cutting speed is 7000rpm, the cutting time is 10min, and it is stored after cutting. It is an anti-shrinkage and anti-pilling wool fabric finishing agent.
Embodiment 2
[0036] (1) Pour 15 parts of sodium tripolyphosphate, 4 parts of coumarin gum, 6 parts of polyethylene glycol, 5 parts of hydroxyethyl methacrylate, and 4 parts of allyl glycidyl ether into the container by weight, Stir for 15 minutes at a rotating speed of 60r / min, and it will be material A after stirring evenly;
[0037] (2) Take 4 parts of N-oleoyl-N-methyl taurate sodium, 6 parts of n-butanol, and 240 parts of water by weight, and mix the ingredients of step (2) in the container evenly, and it is B material ;
[0038] (3) Put the material A that has been stirred evenly in step (1) into material B, and then stir for 10 minutes at a speed of 60r / min, and then use a shearer to shear the mixed solution evenly. The cutting speed is 5000rpm, the shearing time is 5min, and it is stored after shearing. It is an anti-shrinkage and anti-pilling wool fabric finishing agent.
Embodiment 3
[0040] (1) Pour 13 parts of sodium tripolyphosphate, 5 parts of coumarin gum, 4 parts of polyethylene glycol, 10 parts of hydroxyethyl methacrylate, and 6 parts of allyl glycidyl ether into the container by weight, Stir for 5 minutes at a rotational speed of 120r / min, and it will be material A after stirring evenly;
[0041] (2) Take 5 parts of sodium N-oleoyl-N-methyl taurate, 5 parts of n-butanol, and 330 parts of water by weight, and mix the ingredients in step (2) evenly in a container to form material B ;
[0042] (3) Put the material A that has been stirred evenly in step (1) into material B, and then stir for 30 minutes at a speed of 120r / min, and then use a shearer to shear the mixed solution evenly. The cutting speed is 7000rpm, the cutting time is 10min, and it is stored after cutting. It is an anti-shrinkage and anti-pilling wool fabric finishing agent.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com