[0019] The invention discloses a process for manufacturing waste composite flooring. Specifically, the process includes the following steps:
[0020] A. Selection of raw materials: select 50kg shavings and 50kg sawdust as raw materials, remove impurities in the raw materials, and select phenolic glue as auxiliary materials;
[0021] B. Drying and soaking: Dry the shavings and sawdust to control their moisture content to 4%-12%, then pour 50kg of shavings and 50kg of sawdust into the phenolic glue and soak for 2 hours;
[0022] C. Drying: Dry the soaked raw materials to make the water content 6%-10%;
[0023] D. Hot press forming: Put the dried raw materials into the mold cavity of the hot press for hot press forming. The process is as follows: first use low pressure 3.0Mpa hot press for 45 seconds, then use high pressure 6.0Mpa hot press for 3.5 minutes, And control the temperature in the mold cavity to be 160°C during hot pressing, and after the hot pressing is completed, a ...
Embodiment 2
[0032] The invention discloses a process for manufacturing waste composite flooring. Specifically, the process includes the following steps:
[0033] A. Selection of raw materials: select 100kg shavings and 100kg sawdust as raw materials, remove impurities in the raw materials, and select phenolic glue as auxiliary materials;
[0034] B. Drying and soaking: Dry the shavings and sawdust to control their moisture content to 7%-9%, then pour the shavings and sawdust into the phenolic glue according to the ratio of 1:1, and soak for 11 hours;
[0035] C. Drying: drying the soaked raw materials to make the water content 8%;
[0036] D. Hot pressing: Put the dried raw materials into the mold cavity of the hot press for hot pressing. The process is as follows: first use low pressure 3.0Mpa hot pressing for 50 seconds, and then use high pressure 6.0Mpa hot pressing for 4 minutes. And control the temperature in the mold cavity to be 165°C during hot pressing, and after the hot pressin...
Embodiment 3
[0045] The invention discloses a process for manufacturing waste composite flooring. Specifically, the process includes the following steps:
[0046] A. Selection of raw materials: select 150kg shavings and 150kg sawdust as raw materials, remove impurities in the raw materials, and select phenolic glue as auxiliary materials;
[0047] B. Drying and soaking: Dry the shavings and sawdust to control their moisture content to 4%-12%, then pour 50kg of shavings and 50kg of sawdust into the phenolic glue and soak for 20 hours;
[0048] C. Drying: Dry the soaked raw materials to make the water content 10%;
[0049] D. Hot pressing molding: put the dried raw materials into the mold cavity of the hot press machine, and carry out hot pressing molding. The process is as follows: first use low pressure 3.0Mpa hot pressing for 55 seconds, then use high pressure 6.0Mpa hot pressing for 4.5 minutes, And control the temperature in the mold cavity to be 170°C during hot pressing, and after th...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com