Embodiment 1
[0042] Example 1 Preparation of thermal insulation and noise-proof foaming material for tents
[0043] 1) Prepare the adhesive layer coating solution: Weigh the raw materials according to the weight ratio of each component of the adhesive layer coating solution, then put them into the mixer, stir and mix for 20-30 minutes, and obtain the adhesive layer coating solution with a viscosity of 10000-15000 centimeters Park;
[0044] The subbing layer coating liquid comprises the following components by weight:
[0045]
[0046] 2) Preparation of foam layer coating solution: Weigh the raw materials according to the weight ratio of each component of the foam layer, then put them into a mixer, stir and mix for 15-30 minutes, and obtain a foam layer coating solution with a viscosity of 20000-30000 centimeters Poor; among them, the AC foaming agent needs to be ground before use, and the fineness is less than 20 μm.
[0047] The foam layer coating solution comprises the following com...
Embodiment 2
[0056] Example 2 Preparation of thermal insulation and noise-proof foaming material for tents
[0057] 1) Prepare the adhesive layer coating solution: Weigh the raw materials according to the weight ratio of each component of the adhesive layer coating solution, then put them into the mixer, stir and mix for 20-30 minutes, and obtain the adhesive layer coating solution with a viscosity of 10000-15000 centimeters Park;
[0058] The subbing layer coating liquid comprises the following components by weight:
[0059]
[0060] 2) Preparation of foam layer coating solution: Weigh the raw materials according to the weight ratio of each component of the foam layer, then put them into a mixer, stir and mix for 15-30 minutes, and obtain a foam layer coating solution with a viscosity of 20000-30000 centimeters Poor; among them, the AC foaming agent needs to be ground before use, and the fineness is less than 20 μm.
[0061]
[0062] 3) Prepare the coating solution for the treatme...
Embodiment 3
[0068] Example 3 Preparation of thermal insulation and noise-proof foaming material for tents
[0069] 1) Prepare the adhesive layer coating solution: Weigh the raw materials according to the weight ratio of each component of the adhesive layer coating solution, then put them into the mixer, stir and mix for 20-30 minutes, and obtain the adhesive layer coating solution with a viscosity of 10000-15000 centimeters Park;
[0070] The subbing layer coating liquid comprises the following components by weight:
[0071]
[0072] 2) Preparation of foam layer coating solution: Weigh the raw materials according to the weight ratio of each component of the foam layer, then put them into a mixer, stir and mix for 15-30 minutes, and obtain a foam layer coating solution with a viscosity of 20000-30000 centimeters Poor; among them, the AC foaming agent needs to be ground before use, and the fineness is less than 20 μm.
[0073]
[0074] 3) Prepare the coating solution for the treatme...