Embodiment 1
[0063] Embodiment Fibroin hemostatic material
[0064] 1) Preparation of silk fibroin solution
[0065] Put 10 grams of degummed silk in 40ml of 9.3M lithium bromide solution, stir with a glass rod to make the degummed silk fully soaked, put it in a 60°C oven and heat for 4 hours. Using a Pierce dialysis device with a cut-off molecular weight of 3500-10000 Daltons or a common dialysis bag, dialysis for 36 hours and changing the water 7-8 times can remove the lithium bromide component in the solution, while the silk fibroin remains in the dialysis bag.
[0066] Move the silk fibroin solution in the dialysis bag into a centrifuge container, discard the precipitate after centrifugation, and take the upper layer solution which is the silk fibroin solution to be prepared.
[0067] 2) preparation of polyethylene glycol solution
[0068] A polyethylene glycol (PEG) solution with a molecular weight of 1000-10000 is configured into a solution, and the concentration is 1-40wt%.
[00...
Embodiment 2
[0071] Example Two silk fibroin hemostatic material preparation
[0072] Mix the silk fibroin solution with a concentration of 3wt% and polyethylene glycol 2000 (10wt%) at a volume ratio of 10:1-10:3, divide it into containers, and then put it into a freeze dryer for pre-freezing and drying 1. After secondary drying, the freeze-drying process is completed to obtain the silk fibroin hemostatic material.
[0073] Add corresponding ultrapure water according to the content of silk fibroin hemostatic material to obtain a mixed solution of a certain concentration, place it in a constant temperature and humidity incubator at 37°C to form a gel, turn the test tube containing the mixed solution upside down, and take the solution not flowing as an indicator Observe the state of the gel. The final concentration of each silk fibroin is 6% and 12%, take 5 parallel samples, each take 100ul solution and put it in a tensile testing machine to test the solution adhesion in the initial state. ...
Embodiment 3
[0076] Embodiment Three silk fibroin hemostatic film / powder preparation
[0077] Mix the silk fibroin solution with a concentration of 3wt% and polyethylene glycol 4000 (40wt%) at a ratio of 10:0.25-10:3 and distribute them in containers, then put them into a freeze dryer, and pre-freeze, dry, After secondary drying, the freeze-drying process is completed to obtain the silk fibroin hemostatic material.
[0078] Add corresponding ultrapure water according to the content of silk fibroin hemostatic material to obtain a mixed solution with a certain concentration, and place it in a constant temperature and humidity incubator at 37°C to form a gel. The final concentration of each silk fibroin is 6% and 12%, take 5 parallel samples, each take 100ul solution and put it in a tensile testing machine to test the solution adhesion in the initial state. Adhered between two metal sheets, one of the metal sheets is stretched vertically upward at a certain speed, and the maximum required pu...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com