[0020] (1) Preparation solution: Take 1g / L fatty alcohol polyoxyethylene ether, 15g / L anti-felting additive, 3g / L wetting agent, 1g / L hydroxypropyl methylcellulose, 1g / L oligomer Polyhydric alcohol, 4g / L bisulfite, 4-5g / L cross-linking agent, prepare the working solution, add lauric acid to adjust the pH value to 5.5-6.5;
[0021] The solution prepared in step (1) is cooled to below 40°C, and an organic solvent is added to dilute the polyurethane prepolymer;
[0022] (2) Soak the knitted sweater clothes in the above solution, fully soaked and then dry until the liquid-carrying rate of the clothes is 60%;
[0023] (3) Perform wrinkle finishing on the clothes treated in step (2); in the wrinkle finishing, the wrinkle is generated by pressing with an ironing board, and the temperature during the pressing process is 150-160°C, and the time is 30 ~60 seconds; or the wrinkle finishing is pressed by an ironing board at a temperature of 165°C for 20 seconds;
[0024] (4) Rinse the w...
Embodiment 2
[0026] (1) Preparation solution: Take 2g / L fatty alcohol polyoxyethylene ether, 2g / L anti-felting additive, 2g / L wetting agent, 1g / L hydroxypropyl methylcellulose, 1g / L oligomer Polyhydric alcohol, 5.5g / L bisulfite, 4.4g / L cross-linking agent, prepare the working solution, add lauric acid to adjust the pH value to 5.5-6.5;
[0027] The solution prepared in step (1) is cooled to below 40°C, and an organic solvent is added to dilute the polyurethane prepolymer;
[0028] (2) Soak the knitted sweater clothes in the above solution, fully soaked and then dry until the liquid-carrying rate of the clothes is 60%;
[0029] (3) Perform wrinkle finishing on the clothes treated in step (2); in the wrinkle finishing, the wrinkle is generated by pressing with an ironing board, and the temperature during the pressing process is 155° C., and the time is 45 seconds; Or the wrinkle finishing is done by pressing with an ironing board at a temperature of 165°C for 20 seconds;
[0030] (4) Rinse...
Embodiment 3
[0032] (1) Preparation solution: Take 3g / L fatty alcohol polyoxyethylene ether, 25g / L anti-felting additive, 5g / L wetting agent, 1g / L hydroxypropyl methylcellulose, 1g / L oligomer Polyhydric alcohol, 4-7g / L bisulfite, 5g / L cross-linking agent, prepare the working solution, add lauric acid to adjust the pH value to 5.5-6.5;
[0033] The solution prepared in step (1) is cooled to below 40°C, and an organic solvent is added to dilute the polyurethane prepolymer;
[0034] (2) Soak the knitted sweater clothes in the above solution, fully soaked and then dry until the liquid-carrying rate of the clothes is 60%;
[0035] (3) Perform wrinkle finishing on the clothes treated in step (2); in the wrinkle finishing, ironing boards are used to produce wrinkles, and the temperature during the pressing process is 160°C, and the time is 30-60 seconds; or the wrinkle finishing is done by pressing with an ironing board at a temperature of 165°C for 20 seconds;
[0036] (4) Rinse the wrinkled c...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com