A method for judging the pelletizing performance of iron powder ore
A technology of spheroidization index and iron powder, which is applied in the field of discrimination of sintering process conditions, can solve the problem of not being able to truly reflect the size of the adsorption capacity of molecular water and capillary water on the surface of iron ore, not being able to truly reflect iron powder ore, and small specific surface area and other problems, to achieve the effect of simple evaluation method, wide application range and strong operability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0042] Note: The specific iron powder ore is specular iron ore;
[0043] A method for judging the pelletizing performance of iron powder ore, the steps of which are:
[0044] 1) Take 850g of iron powder ore and dry it. The drying temperature is 110°C, and the drying time is 2.5 hours. After testing, the moisture content after drying is 0.042wt%;
[0045] 2) Sieve the iron powder ore after drying, and take the iron powder ore whose particle size is less than 1mm, of which: the amount used to measure the maximum molecular water is 12g, and the amount in the test tube for measuring the maximum capillary water is m a It is 134.1g, and the amount contained in the test tube used for measuring the total pore volume is 5g;
[0046] 3) Determination of maximum molecular water a of iron powder ore with particle size <1mm by centrifugation method:
[0047] A. First, soak 12g of iron powder ore with a particle size of <1mm in water for 12.3 hours;
[0048] B. After soaking, use centrif...
Embodiment 2
[0074] Explanation: The specific iron powder ore is magnetite,
[0075] A method for judging the pelletizing performance of iron powder ore, the steps of which are:
[0076] 1) Take 1000g of iron powder ore and dry it. The drying temperature is 105°C, and the drying time is 4 hours. After testing, the moisture content after drying is 0.009wt%;
[0077] 2) Sieve the iron powder ore after drying, and take the iron powder ore whose particle size is less than 1mm, of which: the amount used to measure the maximum molecular water is 30g, and the amount in the test tube for measuring the maximum capillary water is m a It is 145.7g, and the amount contained in the test tube used for measuring the total pore volume is 4g;
[0078] 3) Determination of the maximum molecular water of iron powder ore with particle size <1mm by centrifugation method:
[0079] A. First, soak 30g of iron powder ore with a particle size of <1mm in water for 18 hours;
[0080] B. After soaking, use centrifug...
Embodiment 3
[0106] Note: The specific iron powder ore is limonite,
[0107] A method for judging the pelletizing performance of iron powder ore, the steps of which are:
[0108] 1) Take 1100g of iron powder ore and dry it. The drying temperature is 107°C, and the drying time is 3 hours. After testing, the moisture content after drying is 0.014wt%;
[0109] 2) Sieve the iron powder ore after drying, and take the iron powder ore whose particle size is less than 1mm, of which: the amount used to measure the maximum molecular water is 25g, and the amount contained in the test tube for measuring the maximum capillary water is 139.4g, The amount contained in the test tube used to measure the total pore volume is 3 g;
[0110] 3) Determination of maximum molecular water a of iron powder ore with particle size <1mm by centrifugation method:
[0111] A. First, soak 25g of iron powder ore with a particle size of <1mm in water for 16 hours;
[0112] B. After soaking, use centrifugal dehydration f...