Supercharge Your Innovation With Domain-Expert AI Agents!

A High Strength and Low Energy Consumption Refining Process for Household Paper

A technology for household paper and low energy consumption, applied in pulp dehydration, pulp property modification, cellulose pulp post-treatment, etc., can solve the problems of insufficient fiber water absorption and swelling, small fiber specific surface area, weak fiber binding force, etc. Achieve the effect of reducing stiffness, reducing fine fiber content and improving paper strength

Active Publication Date: 2021-01-12
CHONGQING LIWEN SANITARY PAPER MFG CO LTD
View PDF9 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

In the prior art, when wood pulp or bamboo pulp is used as the raw material for pulping, the pulping concentration is generally below 10%, the pulp concentration is low, the specific surface area of ​​the fiber is small, the water absorption and swelling of the fiber is not enough and the binding force of the fiber is low. Weak problem, when the pulp enters the refiner for beating in a low-concentration state, the fibers are easily cut off, resulting in the precipitation of a large number of fine fibers, resulting in poor strength of the finished paper, and low-concentration beating consumes a lot of energy

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0025] A high-strength and low-energy consumption household paper refining process of this embodiment comprises the following steps:

[0026] Step a, by mass percentage, 45% bamboo pulp and 55% wood pulp are mixed with pulp, obtain mixed pulp;

[0027] Step b, transport the mixed slurry to the soaking tower with softening liquid to fully soak and moisten it, the soaking time is 24h, and the amount of softening liquid is 20g / L mixed slurry; then wash and dehydrate, separate the softening liquid, and obtain fully runnable slurry;

[0028] The softening liquid is made by mixing the following raw materials in mass percentage:

[0029] Sodium peroxide 15%

[0030] Sodium sulfite 2%

[0031] Disodium EDTA 0.15%

[0032] Sodium di-sec-octyl sulfonate maleate 1.2%

[0033] water balance.

[0034] Step c. The fully moistened slurry is firstly deslagged by a high-concentration slag remover, and then dehydrated by a thickening device to make the concentration of the slurry reach 20...

Embodiment 2

[0038] A high-strength and low-energy consumption household paper refining process of this embodiment comprises the following steps:

[0039] Step a, by mass percentage, 50% bamboo pulp and 50% wood pulp are mixed with pulp, obtain mixed pulp:

[0040] Step b. Transport the mixed slurry to the soaking tower with softening liquid to fully soak and moisten it. The soaking time is 28 hours, and the amount of softening liquid is 16g / L mixed slurry; then wash and dehydrate, separate the softening liquid, and obtain fully runnable slurry;

[0041] The softening liquid is made by mixing the following raw materials in mass percentage:

[0042] Sodium peroxide 17%

[0043] Sodium sulfite 1%

[0044] Disodium EDTA 0.1%

[0045] Sodium di-sec-octyl sulfonate maleate 1.5%

[0046] water balance.

[0047] Step c. The fully moistened slurry is firstly deslagged by a high-concentration slag remover, and then dehydrated by a concentration device to make the concentration of the slurry r...

Embodiment 3

[0051] A high-strength and low-energy consumption household paper refining process of this embodiment comprises the following steps:

[0052] Step a, by mass percentage, 65% bamboo pulp and 35% wood pulp are mixed with pulp, obtain mixed pulp;

[0053] Step b, transport the mixed slurry to the soaking tower with softening liquid to fully soak and moisten it, the soaking time is 36 hours, and the amount of softening liquid is 10g / L mixed slurry; then wash and dehydrate, separate the softening liquid, and obtain fully runnable slurry;

[0054] The softening liquid is made by mixing the following raw materials in mass percentage:

[0055] Sodium peroxide 18%

[0056] Sodium sulfite 3%

[0057] Disodium EDTA 0.25%

[0058] Sodium di-sec-octyl sulfonate maleate 0.5 %

[0059] water balance.

[0060] Step c. The fully moistened slurry is firstly deslagged by a high-concentration slag remover, and then dehydrated by a concentration device to make the concentration of the slurry...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention relates to the technical field of paper-making pulping, in particular to a pulping technology of high-strength low-energy-consumption paper for daily use. The pulping technology comprises the steps that firstly, 45-65% of bamboo pulp and 35-55% of wood pulp are mixed and prepared to obtain mixed pulp, then after being fully soaked and moistened in a pulp soaking tower filled with a softening liquid, the mixed pulp is subjected to slag removal by a high-concentration slag remover, then the concentration of the pulp reaches 20-25% through a concentration device, then the pulp is delivered to a high-concentration pulping machine for pulping, and an enzyme additive is added for high-concentration pulping. The pulping technology of the high-strength low-energy-consumption paper for daily use has the advantages that the prepared pulp makes the paper strength improved significantly, the content of fine fibers in white water is reduced, the fiber loss is reduced, the energy consumption is reduced, the production technology is simple, and the pulping technology is suitable for large-scale industrialized production.

Description

technical field [0001] The invention relates to the technical field of papermaking and pulping, in particular to a high-strength and low-energy consumption household paper refining process. Background technique [0002] The production process of household paper mainly includes a pulping section and a papermaking section. Raw materials are made into pulp with a certain concentration through pulping, desanding, refining and other processes, and then enter the papermaking section of the paper machine through wire pressing and drying. In the prior art, when wood pulp or bamboo pulp is used as the raw material for pulping, the pulping concentration is generally below 10%, the pulp concentration is low, the specific surface area of ​​the fiber is small, the water absorption and swelling of the fiber is not enough and the binding force of the fiber is low. Weak problem, when the pulp enters the refiner for beating under low-concentration state, the fibers are easily cut off, resul...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): D21D1/20D21C5/00D21C9/00D21C9/18D21D5/02D21H11/12
CPCD21C5/005D21C9/002D21C9/18D21D1/20D21D5/02D21H11/12
Inventor 李文俊
Owner CHONGQING LIWEN SANITARY PAPER MFG CO LTD
Features
  • R&D
  • Intellectual Property
  • Life Sciences
  • Materials
  • Tech Scout
Why Patsnap Eureka
  • Unparalleled Data Quality
  • Higher Quality Content
  • 60% Fewer Hallucinations
Social media
Patsnap Eureka Blog
Learn More