Porous heating body, atomizer including porous heating body, and porous body preparation method
A technology of porous heating element and porous body, applied in the field of electronic cigarettes, to achieve the effect of improving replenishment efficiency, reducing conduction, and fast conduction of e-liquid
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0120] Based on the above structure, and based on the idea of improving the overall porosity and smoke output, the present invention further proposes a porous body with higher e-liquid conduction and smoke output efficiency. The preparation method includes the following steps:
[0121] S10, obtain raw materials according to the following components of each mass percentage: 50% to 75% of diatomite, 0% to 10% of alumina, 15% to 35% of pore forming agent, 5% to 10% of clay, and 5% to glass powder 15%;
[0122] S20, mixing the above raw materials with paraffin evenly to make a raw wax block;
[0123] S30, pressing and molding the raw material wax block obtained in step S20 according to the final desired product shape to obtain a green embryo;
[0124] S40, heat the green embryo at 200-500° C. for 4-10 hours, and then sinter at 700-1200° C. for 2-4 hours to obtain a porous body.
[0125] In the above preparation process of the present invention, in step S10, the components sele...
Embodiment 1
[0135] S10, obtaining the following raw material components in various mass percentages: 70g of diatomite, 3g of alumina, 15g of wood fiber pore-forming agent, 5g of clay, and 7g of high-temperature glass powder;
[0136] S11, pour each raw material in step S10 into a planetary ball mill for wet ball milling for 5 hours, and the ball milling medium is deionized water to obtain a uniform mixed powder;
[0137]S20, melting an appropriate amount of paraffin into a liquid state at 80°C, pouring the mixed powder in step S11, cooling while stirring, so that the mixed powder is evenly wrapped with paraffin, and made into a raw material wax cake;
[0138] S30, pour the raw wax cake into the molding machine, control the temperature at 70°C and the pressure at 0.4MPa, and inject the wax cake slurry into the figure 1 In the mold of the corresponding shape of the porous body of the embodiment, a molded green body is obtained;
[0139] S40, the shaped green body is firstly kept at 200° C....
Embodiment 2
[0141] S10, obtaining the following raw material components in various mass percentages: 65g of diatomite, 25g of sucrose pore-forming agent, 5g of clay, and 5g of high-temperature glass powder;
[0142] S11, pour the raw materials in step S10 into a planetary ball mill for wet ball milling for 4 hours, and the ball milling medium is absolute ethanol to obtain a uniform mixed powder;
[0143] S20, melting an appropriate amount of paraffin into a liquid state at 80°C, pouring the mixed powder in step S11, cooling while stirring, so that the mixed powder is evenly wrapped with paraffin, and made into a raw material wax cake;
[0144] S30, pour the raw wax cake into the molding machine, control the temperature at 85°C and the pressure at 1MPa, and inject the wax cake slurry into the figure 1 In the mold of the corresponding shape of the porous body of the embodiment, a molded green body is obtained;
[0145] S40, the molded green body is first kept at 500° C. for 4 hours, and th...
PUM
Property | Measurement | Unit |
---|---|---|
melting point | aaaaa | aaaaa |
melting point | aaaaa | aaaaa |
pore size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com