Embodiment 1
[0031] Taking the production of 1000 grams of the product of the present invention as an example, the raw materials used and the proportioning thereof are:
[0032]
[0033] Product preparation steps:
[0034] (1) After heating the distillate oil to 135°C, add the thermoplastic elastomer and cut it with a high-speed shear for 15 minutes, then continue to stir and develop evenly at 135°C for 3 hours to form a fusion before use;
[0035] (2) Add petroleum resin and epoxy resin to the fusion material to be used in step (1) and mix and stir together for 30 minutes at 135° C. to make them evenly fused, and then keep the temperature at 135° C. for use;
[0036] (3) Add the emulsifier into the water and stir evenly to form a soap solution and heat it to 60°C, then put it into the emulsification equipment for circulation, then add the fusion product to be used in step (2) into the emulsification equipment evenly together with the soap solution The high viscoelastic asphalt road vi...
Embodiment 2
[0038] Taking the production of 1000 grams of the product of the present invention as an example, the raw materials used and the proportioning thereof are:
[0039]
[0040]
[0041] Product preparation steps:
[0042] (1) After heating the distillate oil to 135°C, add the thermoplastic elastomer and cut it with a high-speed shear for 10 minutes, then continue to stir and develop evenly at 135°C for 3 hours to form a fusion before use;
[0043] (2) Add petroleum resin and epoxy resin to the fusion material to be used in step (1) and mix and stir together for 30 minutes at 135° C. to make them evenly fused, and then keep the temperature at 135° C. for use;
[0044] (3) Add the emulsifier into the water and stir evenly to form a soap solution and heat it to 60°C, then put it into the emulsification equipment for circulation, then add the fusion product to be used in step (2) into the emulsification equipment evenly together with the soap solution The high viscoelastic asp...
Embodiment 3
[0046] Taking the production of 1000 grams of the product of the present invention as an example, the raw materials used and the proportioning thereof are:
[0047]
[0048] Product preparation steps:
[0049] (1) After heating the distillate oil to 130°C, add thermoplastic elastomer and cut it with a high-speed shear for 15 minutes, then continue to stir and develop evenly at 130°C for 4 hours to form a fusion before use;
[0050] (2) Add petroleum resin and epoxy resin to the fusion material to be used in step (1) and mix and stir together for 25 minutes at 130°C to make it evenly blend, and then keep it at a temperature of 130°C for use;
[0051] (3) Add the emulsifier into the water and stir evenly to form a soap solution and heat it to 65°C, put it into the emulsification equipment for circulation, and then add the fusion product to be used in step (2) into the emulsification equipment evenly together with the soap solution The high viscoelastic asphalt road viscous l...
PUM
| Property | Measurement | Unit |
|---|---|---|
| softening point | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com