Manufacturing process of self-luminous PVC automobile foot pad
A car mat and manufacturing process technology, which is applied in the field of self-luminous PVC car mat manufacturing technology, can solve the problems of uneven distribution of phosphor powder, affecting the final quality of fluorescent rubber materials, and poor mixing and stirring effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0033] A kind of manufacture technology of self-illuminating PVC car mat, comprises the following steps:
[0034] (1) Proportion the raw materials according to the following parts by weight: configure 80 parts of polyvinyl chloride SG-5, 50 parts of plasticizer (DOP), 1 part of calcium zinc stabilizer, 2,6-ditertbutyl p-methyl 1 part of phenol, 5 parts of luminous powder;
[0035] (2) Pour 80 parts of the above-mentioned polyvinyl chloride SG-5, 50 parts of plasticizer (DOP), 1 part of calcium zinc stabilizer, and 1 part of 2,6-ditert-butyl-p-cresol into a high-speed mixer and stir for 5 minutes , control the stirring temperature to 70°C;
[0036] (3) When the stirring time is 3 minutes, add 3 parts of polyethylene glycol and continue stirring;
[0037] (4) After the stirring is completed, pour 5 parts of luminous powder into the above system and stir for 10 seconds;
[0038] (5) After fully stirring, put the above-mentioned mixed raw materials into the injection molding ma...
Embodiment 2
[0041] A kind of manufacture technology of self-illuminating PVC car mat, comprises the following steps:
[0042] (1) Proportion the raw materials according to the following parts by weight: configure 85 parts of polyvinyl chloride SG-5, 53 parts of plasticizer (DOP), 1 part of calcium zinc stabilizer, 2,6-ditert-butyl p-formaldehyde 1.2 parts of phenol, 5.5 parts of luminous powder;
[0043] (2) Put 80-120 parts of polyvinyl chloride SG-5, 53 parts of plasticizer (DOP), 1 part of calcium zinc stabilizer, and 1.2 parts of 2,6-ditertbutyl p-cresol into a high-speed mixer Stir at medium temperature for 5.5min, and control the stirring temperature to 70-75°C;
[0044] (3) When the stirring time is 3-6 minutes, add 3.3 parts of polyethylene glycol and continue stirring;
[0045] (4) After the stirring is completed, pour 5.5 parts of luminous powder into the above system and stir for 10.5s;
[0046] (5) After the full stirring is completed, put the above-mentioned mixed raw mate...
Embodiment 3
[0049] A kind of manufacture technology of self-illuminating PVC car mat, comprises the following steps:
[0050] (1) Proportion the raw materials according to the following parts by weight: configure 90 parts of polyvinyl chloride SG-5, 55 parts of plasticizer (DOP), 1 part of calcium zinc stabilizer, 2,6-ditertbutyl p-methyl 1.4 parts of phenol, 6 parts of luminous powder;
[0051] (2) Pour 90 parts of the above polyvinyl chloride SG-5, 55 parts of plasticizer (DOP), 1 part of calcium zinc stabilizer, and 1.4 parts of 2,6-ditert-butyl-p-cresol into a high-speed mixer and stir for 6 minutes , control the stirring temperature to 71°C;
[0052] (3) When the stirring time is 4 minutes, add 3.5 parts of polyethylene glycol and continue stirring;
[0053] (4) After the stirring is completed, pour 6 parts of luminous powder into the above system and stir for 11s;
[0054] (5) After fully stirring, put the above-mentioned mixed raw materials into the injection molding machine for i...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com