Phosphorus-fixing and oxygen-releasing material, and preparation method and application thereof
A technology for releasing oxygen and calcium peroxide, which is applied in chemical instruments and methods, water/sludge/sewage treatment, water pollutants, etc. It can solve the problems of submerged plant growth stress, insufficient dissolved oxygen in lakes, and low transparency of lakes, etc. , to achieve the effects of improving the transparency of the lake, restoring the effect and investment, and reducing the preparation cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0044] According to another aspect of the present invention, the present invention relates to a method for preparing a phosphorus-fixing and oxygen-releasing material, comprising the following steps:
[0045] Calcium peroxide, carrier, embedding agent and flocculant are mixed and stirred to obtain a phosphorus-fixing and oxygen-releasing material.
[0046] The preparation method of the phosphorus-fixing and oxygen-releasing material of the invention is simple and easy, and the material with excellent performance can be obtained by mixing and stirring each component.
[0047] Preferably, the stirring time is 6-24h;
[0048] In one embodiment, the stirring time is 6-24 hours, and 8 hours, 10 hours, 12 hours, 15 hours, 18 hours, 20 hours or 22 hours can also be selected.
[0049] Preferably, the stirring time is 12h.
[0050] In a preferred embodiment, the preparation method of the phosphorus-fixing and oxygen-releasing material comprises the following steps:
[0051] (a) putt...
Embodiment 1
[0060] A phosphorus-fixing and oxygen-releasing material, comprising the following components in parts by weight:
[0061] 20 parts of calcium peroxide, 10 parts of kaolin, 15 parts of medical stone, 25 parts of polyvinyl alcohol solution, 20 parts of chitosan and 10 parts of polyacrylamide;
[0062] Wherein, the mass percent of polyvinyl alcohol in the polyvinyl alcohol solution is 10%;
[0063] A preparation method for phosphorus-fixing and oxygen-releasing material, comprising the following steps:
[0064] (a) Put polyvinyl alcohol into distilled water to prepare polyvinyl alcohol solution, the temperature of distilled water is 100°C;
[0065] (b) Calcium peroxide, carrier, polyvinyl alcohol solution and flocculant were mixed and stirred for 12 hours to obtain a phosphorus-fixing and oxygen-releasing material.
Embodiment 2
[0067] A phosphorus-fixing and oxygen-releasing material, comprising the following components in parts by weight:
[0068] 30 parts of calcium peroxide, 10 parts of kaolin, 15 parts of medical stone, 25 parts of polyvinyl alcohol solution, 20 parts of chitosan and 5 parts of polyacrylamide;
[0069] A preparation method for phosphorus-fixing and oxygen-releasing material, comprising the following steps:
[0070] (a) Put polyvinyl alcohol into distilled water to prepare polyvinyl alcohol solution, the temperature of distilled water is 98°C;
[0071] (b) Calcium peroxide, carrier, polyvinyl alcohol solution and flocculant were mixed and stirred for 6 hours to obtain a phosphorus-fixing and oxygen-releasing material.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com