[0014] A kind of preparation technology of 18.5 micron short wool strips comprises the following specific steps:
[0015] 1) Wool selection: 50% lamb wool, 40% weaned lamb wool and 10% early sheared wool;
[0016] 2) Opening, scouring and drying: Opening, scouring and drying the three kinds of wool in step 1) respectively. No lotion is added to the first and last tanks, the cleaning temperature of lambs and weaned lambs is controlled at 35°C, the number of tanks of the scourer is controlled at 4 and the first and last tanks For clean water, add lotion to the rest of the tank; dry the cleaned wool;
[0017] 3) Blending: the dried wool is blended, and the amount of blended wool is 1.1 tons / hour, and blended oil and antistatic agent are added during the blending process, and a sufficient amount of 7KG / T is required for blending the wool;
[0018] 4) Needle front needle combing, combing and back needle process: the traction gauge of the preceding needle comb is 32mm, the speed i...
Embodiment 2
[0021] A kind of preparation technology of 18.5 micron short wool strips comprises the following specific steps:
[0022] 1) Wool selection: 60% lamb wool, 30% weaned lamb wool and 10% early sheared wool;
[0023] 2) Opening, scouring and drying: Opening, scouring and drying the three kinds of wool in step 1) respectively. No lotion is added to the first and last tanks, the cleaning temperature of lambs and weaned lambs is controlled at 40°C, and the number of tanks of the wool scourer is controlled at 5 and the first and last tanks For clean water, add lotion to the rest of the tank; dry the cleaned wool;
[0024] 3) Wool blending: the wool after drying is blended, the amount of blended wool is 1.3 tons / hour, blended wool oil and antistatic agent are added in the wool blending process, and the wool oil needs to be blended in a sufficient amount of 8KG / T;
[0025] 4) Needle front needle combing, combing and back needle process: the traction gauge of the preceding needle comb...
Embodiment 3
[0028] A kind of preparation technology of 18.5 micron short wool strips comprises the following specific steps:
[0029] 1) Wool selection: lamb's wool 55%, weaned lamb's wool 37%, early shearing 8%;
[0030] 2) Opening, scouring and drying: Opening, scouring and drying the three kinds of wool in step 1) respectively, the scouring temperature of the early sheared wool is controlled at 44°C, and the scouring machine is 4 No lotion is added to the first and last tanks, the cleaning temperature of lambs and weaned lambs is controlled at 38°C, and the number of tanks of the scourer is controlled at 5 and the first and last tanks For clean water, add lotion to the rest of the tank; dry the cleaned wool;
[0031] 3) Wool blending: the wool after drying is blended, the amount of blended wool is 1.2 tons / hour, blended wool oil and antistatic agent are added in the wool blending process, and the wool oil needs to be blended in a sufficient amount of 7.5KG / T;
[0032] 4) Needle front...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com