[0045] Mix 1.5 kg of 196# unsaturated polyester resin, 3.7 kg of aluminum hydroxide (toothpaste grade), 0.003 kg of cobalt isozincate, and 0.003 kg of potassium peroxide ethyl ketone. The mold is naturally placed indoors to solidify, and the mold is demoulded after molding. After filling the air bubbles, the imitation jade decorative lines can be obtained.
Embodiment 2
[0047] Mix 1.08 kg of 128# unsaturated polyester resin, 2.513 kg of calcite stone powder, 0.003 kg of black color paste, 0.002 kg of cobalt alkanecyclic acid, and 0.002 kg of potassium peroxide ethyl ketone. In the line mold, it is cured and molded at a room temperature of 36°C, demolded, and the black imitation jade line is obtained after filling air bubbles.
Embodiment 3
[0049] Mix 2.06 kg of 191# unsaturated polyester resin, 6 kg of aluminum hydroxide, 2 kg of dolomite stone powder, 0.021 kg of green color paste, 0.01 kg of cobalt isozincate, and 0.082 kg of potassium peroxide ethyl ketone, and then put them into the The animal mold coated with the release agent is solidified at room temperature and molded for demoulding, and finally the animal-shaped imitation jade product is obtained after filling air bubbles.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap