Method for manufacturing anti-cracking solid wood blue-white porcelain floor
A production method and technology of blue and white porcelain, applied in the direction of floor, building, building structure, etc., can solve the problems of high water absorption, unsatisfactory use effect, and short service life of solid wood floors, and achieve low water absorption and good use effect. , the effect of prolonging the service life
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0035] Embodiment 1: the concrete steps of the manufacture method of anti-cracking solid wood blue and white porcelain floor are as follows:
[0036] ①Dry the solid wood until the moisture content is ≤10%, and process it into billets;
[0037] ② The blank is processed into a solid wood floor;
[0038] 3. the surface of solid wood floor injects kraft glue with the mode that negative pressure vacuum tank injects, obtains A material; The negative pressure of described negative pressure vacuum tank is-5 atmospheric pressure;
[0039] ④Dry material A until the moisture content is ≤10% to obtain material B;
[0040] 5. All the surfaces of B material are injected with kraft glue in the mode of negative pressure vacuum tank injection to obtain C material; the negative pressure of the negative pressure vacuum tank is -5 atmospheres;
[0041] ⑥Dry material C until the moisture content is ≤10% to obtain material D;
[0042] ⑦Sanding or polishing and painting the material D to make the...
Embodiment 2
[0043] Embodiment 2: the concrete steps of the manufacture method of anti-cracking solid wood blue and white porcelain floor are as follows:
[0044] ①Dry the solid wood until the moisture content is ≤10%, and process it into billets;
[0045] ② The blank is processed into a solid wood floor;
[0046] 3. the surface of solid wood floor injects UV paint with the mode that negative pressure vacuum tank injects, gets A material; The negative pressure of described negative pressure vacuum tank is-0.5 atmospheric pressure;
[0047] ④Dry material A until the moisture content is ≤10% to obtain material B;
[0048] 5. All surfaces of B material inject UV paint with the mode that negative pressure vacuum tank injects, get C material; The negative pressure of described negative pressure vacuum tank is-0.5 atmospheric pressure;
[0049] ⑥Dry material C until the moisture content is ≤10% to obtain material D;
[0050] ⑦Sanding or polishing and painting the material D to make the finish...
Embodiment 3
[0051] Embodiment 3: the concrete steps of the manufacture method of anti-cracking solid wood blue and white porcelain floor are as follows:
[0052] ①Dry the solid wood until the moisture content is ≤10%, and process it into billets;
[0053] ② The blank is processed into a solid wood floor;
[0054] 3. the surface of solid wood floor injects calcium carbonate with the mode that negative pressure vacuum tank injects, gets A material; The negative pressure of described negative pressure vacuum tank is-1 atmospheric pressure;
[0055] ④Dry material A until the moisture content is ≤10% to obtain material B;
[0056] 5. All surfaces of B material inject calcium carbonate with the mode that negative pressure vacuum tank injects, get C material; The negative pressure of described negative pressure vacuum tank is-1 atmospheric pressure;
[0057] ⑥Dry material C until the moisture content is ≤10% to obtain material D;
[0058] ⑦Sanding or polishing and painting the material D to m...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com