A body gel water and elastic technology, applied in the direction of multi-color effect coatings, coatings, etc., can solve the problems of complex formulas, insufficient use, and increased production costs, and achieve simple formulas and processes, better and more durable effects, and improved The effect of service life
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0034] 1. Prepare 600 parts of protective colloid solution.
[0035] components
Selected reagents
content
water
water
556 copies
Cationic protective glue
vinyl amide polymer
40 copies
Defoamer
Thick build defoamer
2 copies
fungicide
Isothiazolinone
2 copies
[0036] Method: Mix and stir the above reagents until completely dissolved. Wherein the cationic protective colloid is a vinyl amide polymer with a grafting degree of 1%.
[0037] 2. Prepare 400 parts of elastic paint.
[0038] components
Selected reagents
content
water
water
140 copies
lubricant
BS-100
3 copies
Dispersant
BS-5060
1 copy
Defoamer
BS-154
3 copies
Titanium dioxide
rutile
10 copies
Aluminum silicate
Aluminum silicate
10 copies
Kaolin
Calcined kaolin
20 copies
Hydroxyethyl cellulose
30,0...
Embodiment 2
[0047] 1. Prepare 450 parts of protective colloid solution.
[0048] components
Selected reagents
content
water
water
416 copies
Cationic protective glue
Methacryloxyammonium Chloride Polymer
30 copies
Defoamer
Thick build defoamer
3 copies
fungicide
Isothiazolinone
1 copy
[0049] Method: Mix and stir the above reagents until completely dissolved. Among them, the cationic protective glue is connected
[0050] A methacryloyloxyammonium chloride polymer with a branching degree of 1.5%;
[0051] 2. Prepare 300 parts of elastic paint.
[0052] components
Selected reagents
content
water
water
90 copies
lubricant
BS-100
2 copies
Dispersant
BS-5060
1 copy
Defoamer
BS-154
2 copies
[0053] Titanium dioxide
Titanium dioxide
5 copies
Aluminum silicate
Aluminum silicate
5 copies ...
Embodiment 3
[0062] 1. Prepare 600 parts of protective colloid solution.
[0063] components
Selected reagents
content
water
water
562 copies
Cationic protective glue
Hydroxymethylammonium Chloride Polymer
35 copies
Defoamer
Thick build defoamer
1 copy
fungicide
Isothiazolinone
2 copies
[0064] Method: Mix and stir the above reagents until completely dissolved. Wherein the cationic protective colloid is a hydroxymethyl ammonium chloride polymer, and the degree of grafting is 2.5%;
[0065] 2. Prepare 400 parts of elastic paint.
[0066] components
Selected reagents
content
water
water
108 copies
lubricant
BS-100
3 copies
Dispersant
BS-5060
1 copy
Defoamer
BS-154
1 copy
Titanium dioxide
Titanium dioxide
2 copies
Aluminum silicate
Aluminum silicate
2 copies
Kaolin
Kaolin
80 copies...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
degree of grafting | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap