Process for preparing bamboo rib reinforced composite packaging material by utilizing waste paper and bamboo
A composite packaging material and waste paper technology, applied in paper/cardboard layered products, layered products, chemical instruments and methods, etc., can solve the problems of uneven distribution of bamboo fibers, low utilization rate, and pressure difference, etc. The effect of expanding the scope of application, uniform molecular structure of paper, and stable performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0037] A kind of technology of the waste paper composite packaging material that the bamboo rib that prepares with waste paper, bamboo material strengthens comprises the following steps:
[0038] (1) Preparation of cardboard:
[0039] (11), waste paper pretreatment:
[0040] Firstly, the impurities in the recycled waste paper are removed, the cleaned waste paper is deinked and the pulping method is used to make paper raw material pulp;
[0041] (12) Preparation of mixed pulp:
[0042] Add 7% of flame retardant, 8% of moisture-proof agent, 5% of filler and appropriate amount of anti-mold agent, foaming agent and plasticizer according to the weight of waste paper to the paper raw material slurry, and heat it to 50-80 Stir evenly at ℃ for later use;
[0043] (13), cardboard forming:
[0044] Pour the mixed pulp into a flat mold, press down according to the required thickness and density at 150-170°C, and then dry it after demoulding;
[0045] (2), preparation of bamboo rib r...
Embodiment 2
[0057] A kind of technology of the paper-bamboo composite packaging material that the bamboo rib that prepares with waste paper, bamboo material strengthens, comprises the following steps:
[0058] (1) Preparation of cardboard:
[0059] (11), waste paper pretreatment:
[0060] Firstly, the impurities in the recycled waste paper are removed, the cleaned waste paper is deinked and the pulping method is used to make paper raw material pulp;
[0061] (12) Preparation of mixed pulp:
[0062] Add 7% of flame retardant, 8% of moisture-proof agent, 5% of filler and appropriate amount of anti-mold agent, foaming agent and plasticizer according to the weight of waste paper to the paper raw material slurry, and heat it to 50-80 Stir evenly at ℃ for later use;
[0063] (13), cardboard forming:
[0064] Pour the mixed pulp into a flat mold, press down according to the required thickness and density at 150-170°C, and then dry it after demoulding;
[0065] (2), preparation of bamboo rib...
Embodiment 3
[0075] A kind of technology of the paper-bamboo mixed packing material that the bamboo rib of waste paper, bamboo preparation is strengthened comprises the following steps:
[0076] (1) Preparation of cardboard:
[0077] (11), waste paper pretreatment:
[0078] Firstly, the impurities in the recycled waste paper are removed, the cleaned waste paper is deinked and the pulping method is used to make paper raw material pulp;
[0079] (12) Preparation of mixed pulp:
[0080] Add 7% of flame retardant, 8% of moisture-proof agent, 5% of filler and appropriate amount of anti-mold agent, foaming agent and plasticizer according to the weight of waste paper to the paper raw material slurry, and heat it to 50-80 Stir evenly at ℃ for later use;
[0081] (13), cardboard forming:
[0082] Pour the mixed pulp into a flat mold, press down according to the required thickness and density at 150-170°C, and then dry it after demoulding;
[0083] (2), preparation of bamboo rib reinforcement b...