Smelting residue flash magnetizing roast comprehensive recycling technology
A flash magnetization roasting and magnetization roasting technology, which is applied in the metallurgical industry, can solve the problems of polluting the environment, wasting resources, and having little use value, and achieves the effect of reducing environmental pollution and reducing environmental pollution.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0022] Smelting waste slag flash magnetization roasting comprehensive recycling process, smelting waste slag contains 38% iron, 1.6g / t gold, 37.5g / t silver, -200 mesh ≥ 90%. The smelting waste residue is dried and dispersed to obtain a powdery material with a moisture weight content of 2% and a particle size of 0.074mm ≥ 80%. The powdery material is accurately measured by a quantitative feeding scale and then transported to the preheating system for four-stage preheating. Then it is roasted under the condition of 750°C in a magnetized roaster, and then gas-solid separation, cooling, grinding and grading, concentration, full slime cyanide leaching of gold and silver, and cyanide tailings are magnetically separated to obtain iron concentrate; four of them The conditions for the stage preheating are: the temperature of the stage one preheating is 330°C and the time is 25 seconds; the temperature of the stage two is 530°C and the time is 25 seconds; 25 seconds.
[0023] The outle...
Embodiment 2
[0029] Smelting waste slag flash magnetization roasting comprehensive recycling process, smelting waste slag contains 35.5% iron, 1.46g / t gold, 38.75g / t silver, -200 mesh ≥ 92%. The smelting waste residue is dried and dispersed to obtain a powdery material with a moisture weight content of 2% and a particle size of 0.074mm ≥ 80%. The powdery material is accurately measured by a quantitative feeding scale and then transported to the preheating system for four-stage preheating. It is then roasted in a magnetized roaster at 760°C, then separated from gas and solid, cooled, concentrated after grinding and grading, gold and silver are leached by cyanide leaching, and iron concentrate is obtained from cyanide tailings by magnetic separation; four of them The preheating conditions for the first stage are as follows: the first stage preheating temperature is 340°C, and the time is 20 seconds; the second stage is 550°C, and the time is 20 seconds; 20 seconds; control the outlet tempera...
Embodiment 3
[0035] Smelting waste slag flash magnetization roasting comprehensive recycling process, smelting waste slag contains 36.5% iron, 1.26g / t gold, 31.57g / t silver, -200 mesh ≥ 98.5%. The smelting waste residue is dried and dispersed to obtain a powdery material with a moisture weight content of 2% and a particle size of 0.074mm ≥ 80%. The powdery material is accurately measured by a quantitative feeding scale and then transported to the preheating system for four-stage preheating. Then it is roasted under the condition of 780 ℃ in the magnetized roaster, and then gas-solid separation, cooling, grinding, classification, concentration, cyanide leaching of gold and silver, and magnetic separation of cyanide tailings to obtain iron concentrate; The heating conditions are: the first-level preheating temperature is 350°C, and the time is 20 seconds; the second-level preheating is 540°C, and the time is 20 seconds; the third-level preheating is 720°C, and the time is 20 seconds; the four...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com