Burn-free ceramsite
A technology of ceramsite and aluminum slag powder, applied in the direction of sustainable waste treatment, solid waste management, climate sustainability, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] Unfired ceramsite is prepared from the following components by weight percentage: the amount of aluminum slag powder is 5‰, slag powder is 65%, slag is 25%, desulfurized gypsum is 8%, and the amount of admixture is 1.5%. , The relative humidity is 95% for more than 7 days.
[0016] The apparent density of unfired ceramsite is 550kg / m 3 , Cylinder compressive strength 1.5MPa.
Embodiment 2
[0018] Unfired ceramsite is prepared from the following components by weight percentage: the amount of aluminum slag powder is 7‰, slag powder is 60%, slag is 30%, desulfurization gypsum is 8%, and the amount of admixture is 1.3%. , The relative humidity is 95% for more than 7 days.
[0019] The apparent density of unfired ceramsite is 500kg / m 3 , Cylinder compressive strength 1.3Mpa.
Embodiment 3
[0021] Unfired ceramsite is prepared from the following components by weight percentage: the amount of aluminum slag powder is 3‰, slag powder is 57%, slag is 30%, desulfurization gypsum is 10%, and the amount of admixture is 2.7%. , The relative humidity is 95% for more than 7 days.
[0022] The apparent density of unfired ceramsite is 610kg / m 3 , Cylinder compressive strength 2.0Mpa.
PUM
| Property | Measurement | Unit |
|---|---|---|
| specific surface area | aaaaa | aaaaa |
| density | aaaaa | aaaaa |
| cylinder compressive strength | aaaaa | aaaaa |