Manufacturing method of suede leather polyurethane synthetic leather with high?physical properties
A manufacturing method and synthetic leather technology, applied in textiles and papermaking, fabric surface trimming, roughening, etc., can solve the problems of inferior physical properties, low production efficiency, and long process flow, etc., to achieve a strong surface feel and increase production efficiency , reduce the effect of wet process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A kind of manufacture method of high physical property suede polyurethane synthetic leather, comprises the following steps:
[0019] 1. Preparation of semi-finished synthetic leather: apply polyurethane foam slurry to the base fabric, and then dry it in an oven.
[0020] The polyurethane foam slurry formula is (by weight):
[0021] Foaming resin ST-2030 80 parts
[0022] Protein resin 15 parts
[0023] Dimethylformamide 100 parts
[0024] Foaming agent 920-DU40 1.5 parts
[0025] Foaming agent 920-DU80 2.5 parts
[0026] 12 parts of solvent-based color paste
[0027] Silicone feel agent 1.5 parts.
[0028] Set the temperature of the oven to a certain gradient, the specific temperature is: 80°C, 130°C, 150°C, 130°C, each temperature is baked for 30 seconds in turn, and the foaming process is completed in 2 minutes.
[0029] 2. Sanding treatment: The synthetic leather semi-finished product that has completed the foaming process is first ground with a multi-roller g...
Embodiment 2
[0033] A kind of manufacture method of high physical property suede polyurethane synthetic leather, comprises the following steps:
[0034] 1. Preparation of semi-finished synthetic leather: apply polyurethane foam slurry to the base fabric, and then dry it in an oven.
[0035] The polyurethane foam slurry formula is (by weight):
[0036] Foaming resin ST-2030 80 parts
[0037] 10 servings of protein resin
[0038] Dimethylformamide 100 parts
[0039] Foaming agent 920-DU40 0.5 parts
[0040] Foaming agent 920-DU80 3 parts
[0041] Solvent-based color paste 5 parts
[0042] Silicone feel agent 0.5 part.
[0043] Set the temperature of the oven to a certain gradient, the specific temperature is: 80°C, 130°C, 150°C, 130°C, each temperature is baked for 30 seconds in turn, and the foaming process is completed in 2 minutes.
[0044] 2. Sanding treatment: The synthetic leather semi-finished product that has completed the foaming process is first ground with a multi-roller gr...
Embodiment 3
[0049] A kind of manufacture method of high physical property suede polyurethane synthetic leather, comprises the following steps:
[0050] 1. Preparation of semi-finished synthetic leather: apply polyurethane foam slurry to the base fabric, and then dry it in an oven.
[0051] The polyurethane foam slurry formula is (by weight):
[0052] Foaming resin ST-2030 80 parts
[0053] Protein resin 20 parts
[0054] Dimethylformamide 100 parts
[0055] Foaming agent 920-DU40 1.5 parts
[0056] Foaming agent 920-DU80 4 parts
[0057] 15 parts of solvent-based color paste
[0058] Silicone feel agent 2.5 parts.
[0059] Set the temperature of the oven to a certain gradient, the specific temperature is: 80°C, 130°C, 150°C, 130°C, each temperature is baked for 30 seconds in turn, and the foaming process is completed in 2 minutes.
[0060] 2. Sanding treatment: The synthetic leather semi-finished product that has completed the foaming process is first ground with a multi-roller gri...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com