Rare-earth mineral collecting agent
A collector and mineral technology, applied in the field of rare earth mineral collectors, can solve the problems of poor selectivity, low recovery rate, and many dosing points.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] Weigh 7Kg of C5-9 hydroxamic acid, 1.5Kg of mediylan and C 11-16 Alkane kerosene 1.5Kg; The above-mentioned raw materials are added in the stirred tank successively according to the above-mentioned order, at normal temperature and pressure, under the condition of a stirring speed of 200 rpm, the stirring time is 1.5h to obtain the rare earth mineral collector of the present invention.
[0018] Effect test
[0019] Rare earth ore flotation (Ce, La) 2 o 3 Coarse concentrate: Wet-grind the rare earth ore until the fineness -0.074mm accounts for more than 75%, adjust the pH=9, use the rare earth mineral collector prepared in the previous step for flotation, and add 100g / t to obtain (Ce, La) 2 o 3 Coarse concentrate.
[0020] Comparative test: replace the rare earth mineral collector with hydroxamic acid soap, the addition amount and other steps are the same.
[0021] Xenotime Flotation Y 2 o 3 Coarse concentrate: wet-grind xenotime until the fineness -0.074mm accoun...
Embodiment 2
[0024] Weigh C 5-9 Hydroxamic acid 7.5Kg, Medialan 1.0Kg and C 11-16 Alkane kerosene 1.5Kg; The above-mentioned raw materials are added in the stirred tank successively according to the above-mentioned order, and at normal temperature and pressure, under the condition of a stirring speed of 200 rpm, the stirring time is 1h to obtain the rare earth mineral collector of the present invention.
[0025] Effect test:
[0026] Rare earth ore flotation (Ce, La) 2 o 3 Coarse concentrate: use the rare earth mineral collector prepared in this example, the addition amount is 80g / t, and the rest of the steps are the same as in Example 1 Rare earth ore flotation (Ce, La) 2 o 3 Coarse concentrate test.
[0027] Xenotime Flotation Y 2 o 3 Coarse concentrate: use the rare earth mineral collector prepared in this embodiment, the addition amount is 80g / t, the steps are the same as the xenotime flotation Y in embodiment 1 2 o 3 Coarse concentrate test.
Embodiment 3
[0029] Weigh C 5-9 Hydroxamic acid 8Kg, Medialan 1.0Kg and C 11-16 Alkane kerosene 1.0Kg; The above-mentioned raw materials are added in the stirred tank successively according to the above order, at normal temperature and pressure, under the condition of a stirring speed of 200 rpm, and a stirring time of 1.2h to obtain the rare earth mineral collector of the present invention.
[0030] Rare earth ore flotation (Ce, La) 2 o 3 Coarse concentrate: use the rare earth mineral collector prepared in this example, the addition amount is 120g / t, and the rest of the steps are the same as in Example 1 Rare earth ore flotation (Ce, La) 2 o 3 Coarse concentrate test.
[0031] Xenotime Flotation Y 2 o 3 Coarse concentrate: use the rare earth mineral collector prepared in this embodiment, the addition amount is 120g / t, the steps are the same as the xenotime flotation Y in embodiment 1 2 o 3 Coarse concentrate test.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com