A water-dispersible fluorescent polymer nanoparticle with pH value and mercury ion ratio detection function, preparation method and application
A technology of fluorescent polymers and nanoparticles, applied in chemical instruments and methods, fluorescence/phosphorescence, luminescent materials, etc., to achieve the effects of increasing accuracy, eliminating measurement errors, and simple synthesis routes
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0026] Embodiment 1: A kind of preparation method of the water-dispersible fluorescent polymer nanoparticle that has pH value and mercury ion ratio detection function, comprises the following steps:
[0027] (1) Miniemulsion polymerization to prepare fluorescent polymer nanoparticles containing EANI.
[0028]Stir the mixture of 0.5g methyl methacrylate, 0.08g AEMH, 0.025g AIBN, 0.075g n-hexadecane and 0.001g EANI on a common magnetic stirrer for 5 minutes to obtain solution a; Ammonium bromide was added to 10ml of water, and stirred on a common magnetic stirrer for 10 minutes to obtain solution b. After mixing the solutions a and b, the pre-emulsion was obtained after stirring at room temperature for 5 minutes. Put the pre-emulsion into a 650W ultrasonic cell pulverizer under an ice-water bath (keep below 20°C), and ultrasonically emulsify for 15 minutes to obtain a stable microemulsion. The mini-emulsion was transferred to a 25ml round bottom flask, and the round bottom fla...
Embodiment 2
[0031] Embodiment 2: A kind of preparation method of the water-dispersible fluorescent polymer nano-particle that has pH value and mercury ion ratio detection function, comprises the following steps:
[0032] (1) Miniemulsion polymerization to prepare fluorescent polymer nanoparticles containing EANI.
[0033] Stir the mixture of 0.5g methyl methacrylate, 0.04g AEMH, 0.025g AIBN, 0.075g n-hexadecane and 0.002g EANI on a common magnetic stirrer for 5 minutes to obtain solution a; Ammonium bromide was added to 10ml of water, and stirred on a common magnetic stirrer for 10 minutes to obtain solution b. After mixing the solutions a and b, the pre-emulsion was obtained after stirring at room temperature for 5 minutes. Put the pre-emulsion into a 650W ultrasonic cell pulverizer under an ice-water bath (keep below 20°C), and ultrasonically emulsify for 15 minutes to obtain a stable microemulsion. The mini-emulsion was transferred to a 25ml round bottom flask, and the round bottom f...
Embodiment 3
[0036] Embodiment 3: A kind of preparation method of the water-dispersible fluorescent polymer nano-particle that has pH value and mercury ion ratio detection function, comprises the following steps:
[0037] (1) Miniemulsion polymerization to prepare fluorescent polymer nanoparticles containing EANI.
[0038] Stir the mixture of 0.5g methyl methacrylate, 0.12g AEMH, 0.025g AIBN, 0.075g n-hexadecane and 0.0015g EANI on a common magnetic stirrer for 5 minutes to obtain solution a; Ammonium bromide was added to 10ml of water, and stirred on a common magnetic stirrer for 10 minutes to obtain solution b. After mixing the solutions a and b, the pre-emulsion was obtained after stirring at room temperature for 5 minutes. Put the pre-emulsion into a 650W ultrasonic cell pulverizer under an ice-water bath (keep below 20°C), and ultrasonically emulsify for 15 minutes to obtain a stable microemulsion. The mini-emulsion was transferred to a 25ml round bottom flask, and the round bottom ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com