Multi-band machine-readable fluorescent anti-counterfeiting ink composition and its application
An anti-counterfeit ink and multi-band technology, which is applied in the direction of ink, application, household appliances, etc., can solve the problems of increasing the cost of the instrument and the difficulty of production
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0047] Weight percentage of offset printing ink:
[0048]
[0049] in:
[0050] The optical characteristic material is YVO 4 :0.1Ce,0.01Nd;
[0051] The linking material, based on the total weight of the linking material, consists of the following components in weight percentage:
[0052] (a) Resin 56%
[0053] (b) Solvent 4%
[0054] (c) Vegetable oil 40%
[0055] in:
[0056] (a) The resin is a rosin-modified phenolic resin, which can be prepared by the technology disclosed in the patent of "Rosin-modified phenolic resin and its preparation method" (publication number: CN103865019A, publication date: June 18, 2014);
[0057] (b) The solvent is 210# mineral oil;
[0058] (c) The vegetable oil is linseed oil
[0059] The pigment is permanent yellow 2G;
[0060] The auxiliary agent is carnauba wax;
[0061] Put the above-mentioned ink raw materials into a container, use a stirring device to stir evenly to a paste dispersion, and use an ink pad to roll the dispersio...
Embodiment 2
[0064] Photocurable screen ink weight percent:
[0065] Optical properties material 0.1%
[0066] Binder 92%
[0067] Auxiliary 7.9%
[0068] in:
[0069] The optical characteristic material is YAP: 0.2Ce, 0.002Yb, 0.05Nd, 0.2Er;
[0070] The linking material is composed of the following components by weight fraction:
[0071] (a):(b):(c):(d)=18:3:6:65=6:1:2:22;
[0072] in:
[0073] (a) is polyurethane acrylate resin (ALLNEX EBECRYL 8402)
[0074] (b) is epoxy acrylate resin (ALLNEX company EBECRYL 650)
[0075] (c) is methacrylic resin (ALLNEX EBECRYL 168)
[0076] (d) Ethoxy ethyl propionate (ALLNEX EBECRYL 110)
[0077] The auxiliary agent is a mixture of silicon dioxide (Cabot company M-5), polysiloxane (Huaxia auxiliary agent HX-2086) and benzoylphenyl phosphite (BASF Lucirin TPO-L), and the weight ratio is:
[0078] Silicon oxide: polysiloxane: benzoyl phenyl phosphite = 2: 0.9: 5 = 1: 4.5: 2.5;
[0079] Put the above-mentioned ink raw materials into a contai...
Embodiment 3
[0081] Embossed ink composition weight percent:
[0082]
[0083] in:
[0084] The optical characteristic material is YAG: 0.05Ce, 0.05Yb, 0.05Er;
[0085] The linking material, based on the total weight of the linking material, consists of the following components in weight percentage:
[0086] (a) Resin 48%
[0087] (b) Vegetable oil 52%
[0088] in:
[0089] (a) The resin is an alkylphenol phenolic resin, which can be prepared by using the technology disclosed in the patent of "thermoplastic mixed alkylphenol phenolic resin for ink and its preparation method" (publication number: CN101597363B, publication date: June 01, 2011);
[0090] (b) vegetable oil is linoleum;
[0091] The pigment is fast yellow;
[0092] The auxiliary agent is carnauba wax;
[0093] Put the above-mentioned ink raw materials into a container, use a stirring device to stir evenly to a paste-like dispersion, and use an ink pad to roll the dispersion to obtain an anti-counterfeiting ink composi...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com