A kind of direct and reverse flotation process for manganese low-grade phosphate rock demanganization
A positive and negative flotation, low-grade technology, applied in flotation, solid separation, etc., can solve the problems of lower quality and production capacity, complex mosaic relationship, and affect the granulation of ammonium phosphate, so as to improve the utilization rate and overcome the The effect of technical difficulties
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0032] A kind of direct and reverse flotation process of manganese low-grade phosphate rock demanganization, its flow chart is shown in figure 1 , the manganese low-grade phosphate rock used is a manganese low-grade phosphate rock in Hubei, and its main chemical composition is:
[0033] Element type
P 2 o 5
MgO
Fe 2 o 3
Al 2 o 3
CaO
SiO 2
Na 2 o
K 2 o
MnO 2
CO 2
F
TiO 2
content / %
10.62
1.96
2.37
3.18
4.68
14.78
30.28
0.40
3.05
31.53
0.07
0.34
[0034] Specific steps are as follows:
[0035]Crush manganese low-grade phosphate rock (raw ore) to -2mm, and then use a grinder to grind the ore until the mass fraction of ore particles with a grinding fineness of -0.074mm accounts for about 68.6%, and then add water to adjust the slurry to the slurry The solid concentration in the medium is 340g / L, and then flows into the mixing tank, and sodium carbonate (3...
Embodiment 2
[0039] A manganese low-grade phosphate rock flotation process, the specific steps are as follows:
[0040] Manganese low-grade phosphate rock (raw ore, composition is the same as in Example 1) is crushed to -2 mm, and then the ore is ground by a grinder until the mass fraction of ore particles with a grinding fineness of -0.074 mm accounts for about 68%. Then add water to adjust the slurry until the solid concentration in the slurry is 340g / L, then flow into the mixing tank, add sodium carbonate (3.5kg / t relative to the amount of raw ore) and water glass (0.8kg / t relative to the amount of raw ore) into the slurry ) to adjust the pH value of the pulp to 10.0, and then add inhibitors (it is formed by mixing carbonate inhibitor NO-2 and dextrin, the ratio of NO-2 to the raw ore is 0.8kg / t, and the ratio of dextrin to the raw ore 0.8kg / t) and positive flotation collector (anionic fatty acid (soap) collector TX-1, the ratio of the dosage to the raw ore is 0.7kg / t) for pulping, the ...
Embodiment 3
[0044] A manganese low-grade phosphate rock flotation process, the specific steps are as follows:
[0045] Crush manganese low-grade phosphate rock (raw ore) to -2mm, and then use a grinder to grind the ore until the mass fraction of ore particles with a grinding fineness of -0.074mm accounts for about 68%, and then add water to adjust the slurry to the slurry The solid concentration in the medium is 340g / L, and then flows into the mixing tank, and sodium carbonate (4kg / t relative to the amount of raw ore) and water glass (0.7kg / t relative to the amount of raw ore) are added to the pulp to adjust the pH value of the pulp 10.5, then add the inhibitor (it is mixed by carbonate inhibitor NO-2 and dextrin, the ratio of NO-2 to the original ore is 0.6kg / t, and the ratio of dextrin to the original ore is 0.6kg / t) and normal The flotation collector (anionic fatty acid (soap) collector TX-1, the ratio of dosage to the raw ore is 0.8kg / t) is used for pulping, and the temperature of the...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology