Method for preparing and processing semi-worsted section color slub yarn
A processing method and technology of slub yarn, applied in the field of textile yarn, can solve problems such as color, single component, and inability to weave high-grade textile fabrics, etc., and achieve the effect of strong irregularity, unique style and rich colors
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0018] The preparation and processing method of a kind of semi-worsted section colored slub yarn described in this embodiment, the steps are as follows:
[0019] The first step is the selection of raw materials: 100% 80S merino wool;
[0020] The second step, dyeing treatment: mix Merino wool at room temperature with a bath ratio of 1:9, and add 0.8g / L of glacial acetic acid, 0.8g / L of leveling agent Abaig B and the amount added Use reactive dyes for 2% wool from light to dark, and keep it for 10 minutes, then raise the temperature at 0.8°C per minute to 50°C, then raise the temperature at 1°C per minute to 85°C, and keep it for 50 minutes, then stop the temperature rise to make it Cool down to 70°C at 0.8°C per minute and keep it for 5 minutes, then cool down to 50°C at 1°C per minute, and finally cool down naturally to complete the dyeing process, and keep the pH value at 5 throughout the dyeing process; After dyeing, the PH value is 6, that is, the PH value of Merino wool ...
Embodiment 2
[0027] The preparation and processing method of a kind of semi-worsted section colored slub yarn described in this embodiment, the steps are as follows:
[0028] The first step is the selection of raw materials: 100% 90S mercerized merino wool;
[0029] The second step, dyeing treatment: mix mercerized merino wool at room temperature with a bath ratio of 1:9, and add 0.8g / L glacial acetic acid, 0.8g / L leveling agent Abaig B and add The amount is 2% reactive dyes for wool from light to dark, and keep it for 10 minutes, then increase the temperature at 0.8°C per minute to 50°C, then increase the temperature at 1°C per minute to 85°C, and keep it for 50 minutes, then stop the temperature rise, so that It cools down to 70°C at 0.8°C per minute and keeps it for 5 minutes, then cools down to 50°C at 1°C per minute, and finally cools naturally to complete the dyeing process, and the pH value is kept at 5 throughout the dyeing process; Mercerized Merino The PH value of wool after dye...
Embodiment 3
[0036] The preparation and processing method of a kind of semi-worsted section colored slub yarn described in this embodiment, the steps are as follows:
[0037] The first step is the selection of raw materials: 50% 70S mercerized merino wool and 50% cotton fiber;
[0038] The second step, dyeing treatment: mix Merino wool at room temperature with a bath ratio of 1:9, and add 0.8g / L of glacial acetic acid, 0.8g / L of leveling agent Abaig B and the amount added Use reactive dyes for 2% wool from light to dark, and keep it for 10 minutes, then raise the temperature at 0.8°C per minute to 50°C, then raise the temperature at 1°C per minute to 85°C, and keep it for 50 minutes, then stop the temperature rise to make it Cool down to 70°C at 0.8°C per minute and keep it for 5 minutes, then cool down to 50°C at 1°C per minute, and finally cool down naturally to complete the dyeing process, and keep the pH value at 5 throughout the dyeing process; After dyeing, the PH value is 6, that is,...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com