Water-based silver ink and preparation method thereof
A water-based, silver ink technology, applied in ink, household utensils, applications, etc., can solve the problems of silver ink inflation, precipitation and agglomeration, slow drying of deep printing, poor wettability of silver paste, etc. Stability and quality, the effect of improving stability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0034] A water-based silver ink, in parts by mass, comprising the following components: 30 parts of silver paste, 42 parts of water-based binder, 5 parts of anti-wear agent, 2 parts of wetting agent, 1 part of defoamer, 10 parts of alcohol and 10 parts of water.
[0035] The preparation method of water-based silver ink is as follows:
[0036] a. In a dust-free workshop with a temperature of 25°C and a humidity of 50%, mix the wetting agent, alcohol and water to form a mixed solvent;
[0037] b. Soak the silver paste for 120 min with the mixed solvent prepared in step a;
[0038] c. Add the water-based binder to the immersed silver paste prepared in step b, stir, and add the defoamer and the anti-wear agent during the stirring process, and the water-based silver ink is obtained after the stirring is completed. Among them, the stirring speed is 800r / min, and the stirring time is 60min.
[0039] The color phase of the prepared water-based silver ink is determined to have a solid content ...
Embodiment 2
[0043] A water-based silver ink, in parts by mass, comprising the following components: 25 parts of silver paste, 35 parts of water-based binder, 4 parts of anti-wear agent, 1.5 parts of wetting agent, 0.5 parts of defoamer, 17 parts of alcohol and 17 parts of water.
[0044] The preparation method of water-based silver ink is as follows:
[0045] a. In a dust-free workshop with a temperature of 25°C and a humidity of 50%, mix the wetting agent, alcohol and water to form a mixed solvent;
[0046] b. Soak the silver paste for 120 min with the mixed solvent prepared in step a;
[0047] c. Add the water-based binder to the immersed silver paste prepared in step b, stir, and add the defoamer and the anti-wear agent during the stirring process, and the water-based silver ink is obtained after the stirring is completed. Among them, the stirring speed is 1000r / min, and the stirring time is 40min.
[0048] The color phase of the prepared water-based silver ink is determined to have a solid co...
Embodiment 3
[0052] A water-based silver ink, in parts by mass, comprising the following components: 20 parts of silver paste, 38 parts of water-based binder, 0.5 parts of anti-wear agent, 0.2 parts of wetting agent, 0.2 parts of defoamer, 20 parts of alcohol and 20 parts of water.
[0053] The preparation method of water-based silver ink is as follows:
[0054] a. In a dust-free workshop with a temperature of 25°C and a humidity of 60%, mix the wetting agent, alcohol and water uniformly to form a mixed solvent;
[0055] b. Soak the silver paste for 120 min with the mixed solvent prepared in step a;
[0056] c. Add the water-based binder to the immersed silver paste prepared in step b, stir, and add the defoamer and the anti-wear agent during the stirring process, and the water-based silver ink is obtained after the stirring is completed. Among them, the stirring speed is 900r / min, and the stirring time is 50min.
[0057] The color phase of the prepared water-based silver ink is determined to have...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com