[0020] A kind of softening treatment method of willow bark for wicker, comprises the steps:
[0021] (1) Peeling treatment:
[0022] Deleafing and peeling the freshly harvested willow willow, then soaking and cleaning it in a sodium hydroxide solution with a mass fraction of 2% for 30 minutes, taking it out, and finally rinsing it with clean water once before setting aside;
[0023] (2) Poaching treatment:
[0024] Put the Qi Liu treated in step (1) into the treatment liquid, heat to keep the temperature of the treatment liquid at 80°C, boil it in water, and remove the Qi Liu after 40 minutes for later use; the substances in the treatment liquid and their weight percentages It is: 1% hydrophilic silicone oil, 0.2% dibutyl phthalate, 0.1% glycerol, 0.2% 3-aminopropyltriethoxysilane, and the balance is water;
[0025] (3) Microwave treatment:
[0026] The willows treated in step (2) are bundled with 20 pieces, first tied with thin ropes, and then wrapped with polyvinyl chlori...
Embodiment 2
[0031] A kind of softening treatment method of willow bark for wicker, comprises the steps:
[0032] (1) Peeling treatment:
[0033] Deleafing and peeling the freshly harvested willow willows, then soaking and cleaning them in a sodium hydroxide solution with a mass fraction of 2.5% for 35 minutes, taking them out, and finally rinsing them with clean water for later use;
[0034] (2) Poaching treatment:
[0035] Put the Qi Liu treated in step (1) into the treatment liquid, heat to keep the temperature of the treatment liquid at 82°C, boil it in water, and remove the Qi Liu after 43 minutes for later use; each substance in the treatment liquid and its weight percentage It is: 1.2% hydrophilic silicone oil, 0.3% dibutyl phthalate, 0.2% glycerol, 0.4% 3-aminopropyltriethoxysilane, and the balance is water;
[0036] (3) Microwave treatment:
[0037] The willows treated in step (2) are bundled with 27 pieces, first tied with thin ropes, and then wrapped with polyvinyl chloride f...
Embodiment 3
[0042] A kind of softening treatment method of willow bark for wicker, comprises the steps:
[0043] (1) Peeling treatment:
[0044] Deleafing and peeling the freshly harvested willow bark willow, then soaking and cleaning it in a sodium hydroxide solution with a mass fraction of 3% for 40 minutes, taking it out, and finally rinsing it with clean water for later use;
[0045] (2) Poaching treatment:
[0046] Put the Qi Liu treated in step (1) into the treatment liquid, heat to keep the temperature of the treatment liquid at 85°C, boil it in water, and remove the Qi Liu after 45 minutes for later use; each substance in the treatment liquid and its weight percentage It is: 1.5% hydrophilic silicone oil, 0.4% dibutyl phthalate, 0.3% glycerol, 0.5% 3-aminopropyltriethoxysilane, and the balance is water;
[0047] (3) Microwave treatment:
[0048] The willows treated in step (2) are bundled with 30 pieces, first tied with thin ropes, and then covered with polyvinyl chloride film ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction