Fastener steeping liquid, silver-edge-filiform circled fastener and manufacturing method of silver-edge filiform circled fastener
A dipping solution and button technology, which is applied in the field of silver-edged thread-shaped encircled twist buttons and its preparation, and button dipping solution, can solve the problems of low product grade, high cost, and high energy consumption, and achieve simple operation, less process, The effect of low energy consumption
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0038] The present invention has no special limitation on the preparation method of the button dipping liquid, and it can be prepared by adopting the technical scheme of uniformly mixing each formula component well-known to those skilled in the art.
[0039] The present invention also provides a method for preparing a silver-edged wire-shaped encircling button, comprising the following steps:
[0040] a) Soak the blank button in the button dipping solution described in the above technical solution to obtain the button after dipping treatment;
[0041] b) Washing, drying and dry-rolling the buttons obtained in step a) after the impregnation treatment in sequence to obtain silver-edged wire-shaped encircling buttons.
[0042] In the present invention, firstly, the rough button is soaked in the button dipping solution described in the above technical solution to obtain the dipped button. In the present invention, the rough button is preferably selected from a rough horn button o...
Embodiment 1
[0057] (1) Prepare button dipping solution: 1000g water, 20g sodium metasilicate, 120g calcium chloride, 60g calcium hypochlorite, 5g sodium hydroxide and 1g fatty acid methyl ester and condensate of ethylene oxide are mixed uniformly to obtain Button dipping solution;
[0058] (2) After the rough horn button is subjected to water tumbling polishing for 2 hours, it is placed in a nylon mesh bag, and then the nylon mesh bag with the rough horn button is immersed in the button dipping solution obtained in step (1), soaked at 35 ° C for 3 hours, During the soaking process, the nylon mesh bag is kept reciprocating horizontally to obtain the horn buttons after dipping treatment;
[0059] (3) Rinse the ox horn buttons after the dipping treatment obtained in step (2) with clear water, then rinse them with 0.5% acetic acid solution for 3 minutes, spread them on bamboo mats, and dry them at 30°C and 70% relative humidity. Dry in the shade for 24 hours in the shade, and finally dry-rol...
Embodiment 2
[0061] (1) Preparation of button dipping solution: 1000g water, 10g sodium metasilicate, 100g calcium chloride, 50g calcium hypochlorite, 3g sodium hydroxide and 1g fatty acid methyl ester and condensate of ethylene oxide are mixed uniformly to obtain Button dipping solution;
[0062] (2) After the rough horn button is subjected to water tumbling polishing for 2 hours, it is placed in a nylon mesh bag, and then the nylon mesh bag containing the rough horn button is immersed in the button dipping solution obtained in step (1), soaked at 35 ° C for 5 hours, During the soaking process, the nylon mesh bag is kept reciprocating horizontally to obtain the horn buttons after dipping treatment;
[0063] (3) Rinse the ox horn buttons after the dipping treatment obtained in step (2) with clear water, then rinse them with 0.5% acetic acid solution for 3 minutes, spread them on bamboo mats, and dry them at 30°C and 70% relative humidity. Dry in the shade for 24 hours in the shade, and fi...