Embodiment 1
[0044] A kind of preparation method of anti-allergic bioactive glass powder provided in this embodiment, it comprises the following steps:
[0045] (1) the concentrated nitric acid of 6ml 69wt.% is dispersed in 250ml deionized water, stirs, obtains dilute nitric acid;
[0046] (2) Get 125g ethyl orthosilicate and dissolve in dilute nitric acid, stir and hydrolyze for 1.5 hours;
[0047] (3) 10 g of triethyl phosphate was dissolved in the solution obtained in step (2), stirred and hydrolyzed for 0.8 hours;
[0048] (4) Get 62.5g calcium nitrate tetrahydrate and be dissolved in the solution gained in step (3), stir and hydrolyze for 15 minutes;
[0049] (5) Get 700g sodium nitrate, be dissolved in the solution gained in step (4), stir and hydrolyze for 30 minutes;
[0050](6) Place the solution obtained in step (5) at room temperature to age for 20 hours, the solution gradually forms a gel, and continue to age the gel at 60-70°C for 20 hours;
[0051] (7) drying the gel obtai...
Embodiment 2
[0058] The preparation method of the anti-allergic bioactive glass powder provided in this embodiment comprises the following steps:
[0059] (1) disperse the concentrated nitric acid of 8ml 69wt.% in 250ml deionized water, stir, obtain dilute nitric acid;
[0060] (2) Get 160g ethyl orthosilicate and dissolve in dilute nitric acid, stir and hydrolyze for 0.5 hour;
[0061] (3) 14g of triethyl phosphate was dissolved in the solution obtained in step (2), stirred and hydrolyzed for 0.6 hour;
[0062] (4) Get 54g calcium nitrate tetrahydrate and be dissolved in the solution gained in step (3), stir and hydrolyze for 5 minutes;
[0063] (5) Get 300g sodium nitrate and 300g potassium nitrate, be dissolved in the solution gained in step (4), stir and hydrolyze for 20 minutes;
[0064] (5.1) Get 15g citric acid and be dissolved in the solution gained in step (5), stir and hydrolyze for 15 minutes;
[0065] (6) Place the solution obtained in step (5) at room temperature to age for...
Embodiment 3
[0073] The preparation method of the anti-allergic bioactive glass powder provided in this embodiment comprises the following steps:
[0074] (1) the concentrated nitric acid of 10ml 69wt.% is dispersed in 250ml deionized water, stirs, obtains dilute nitric acid;
[0075] (2) Get 195g ethyl orthosilicate and dissolve in dilute nitric acid, stir and hydrolyze for 2 hours;
[0076] (3) 18g of triethyl phosphate was dissolved in the solution obtained in step (2), stirred and hydrolyzed for 0.7 hour;
[0077] (4) Get 105.5g calcium nitrate tetrahydrate and be dissolved in the solution gained in step (3), stir and hydrolyze for 12 minutes;
[0078] (5) Get 500g sodium nitrate and 100g potassium nitrate, be dissolved in the solution gained in step (4), stir and hydrolyze for 5 minutes;
[0079] (6) Place the solution obtained in step (5) at room temperature to age for 24 hours, the solution gradually forms a gel, and continue to age the gel at 60-70°C for 24 hours;
[0080] (7) d...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com