Mildewroof and anti-corrosion treatment process for wood product
A technology for anti-corrosion treatment and wood products, which is applied in the direction of wood treatment, wood treatment details, manufacturing tools, etc. It can solve the problems of cumbersome operation steps and integrity damage, and achieve the effect of simple operation, low cost and improved anti-corrosion performance.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A wood product anti-mildew and anti-corrosion treatment process, comprising the following steps:
[0019] (1) Grind the surface of the processed wood products with different types of sandpaper for 3 times, each time not less than 30 minutes;
[0020] (2) Place the polished wood product in an environment with a temperature of 60°C and a relative air humidity of 75% for 2 hours;
[0021] (3) The above-mentioned treated wood products are modified with a modifier. After mixing the wood products and the modifier in a mass ratio of 1:10, soak for 1 hour, then filter, wash with deionized water, and dry until constant weight;
[0022] (4) Apply paint to the surface of the modified wood product.
[0023] Further, in the step (1), use different types of sandpaper for grinding three times, and use 300# sandpaper, 800# sandpaper and 1200# sandpaper for grinding treatment in sequence.
[0024] Further, after three times of sanding with different types of sandpaper in step (1), so...
Embodiment 2
[0032] A wood product anti-mildew and anti-corrosion treatment process, comprising the following steps:
[0033] (1) Grind the surface of the processed wood products with different types of sandpaper for 3 times, each time not less than 30 minutes;
[0034] (2) Place the polished wood product in an environment with a temperature of 75°C and a relative air humidity of 75% for 2 hours;
[0035] (3) The above-mentioned treated wood products are modified with a modifier. After mixing the wood products and the modifier at a mass ratio of 1:10, soak for 1.5 hours, then filter, wash with deionized water, and dry until constant weight;
[0036] (4) Apply paint to the surface of the modified wood product.
[0037] Further, in the step (1), use different types of sandpaper for grinding three times, and use 300# sandpaper, 800# sandpaper and 1200# sandpaper for grinding treatment in sequence.
[0038] Further, after three times of sanding with different types of sandpaper in step (1),...
Embodiment 3
[0046] A wood product anti-mildew and anti-corrosion treatment process, comprising the following steps:
[0047] (1) Grind the surface of the processed wood products with different types of sandpaper for 3 times, each time not less than 30 minutes;
[0048] (2) Place the polished wood product in an environment with a temperature of 65°C and a relative air humidity of 75% for 2 hours;
[0049] (3) The above-mentioned treated wood products are modified with a modifier. After mixing the wood products and the modifier in a mass ratio of 1:10, soak for 1.2 hours, then filter, wash with deionized water, and dry until constant weight;
[0050] (4) Apply paint to the surface of the modified wood product.
[0051] Further, in the step (1), use different types of sandpaper for grinding three times, and use 300# sandpaper, 800# sandpaper and 1200# sandpaper for grinding treatment in sequence.
[0052] Further, after three times of sanding with different types of sandpaper in step (1),...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com