Method for making iron plate enamel decorative painting
A production method and decorative painting technology, applied in the field of metal enamel, can solve the problems of easy fading and peeling of single-sided tape, affecting the appearance of buildings, affecting the glazing of surface glaze layers, etc., so as to reduce the flattening process of enamel plates and smooth the surface of prints Wrinkle-free and easy-to-control firing temperature
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] A method for making an iron plate enamel decorative painting, comprising the following steps:
[0028] Step 1, select the iron plate, and use a sandblasting and dust removal machine to sandblast and derust the surface of the iron plate;
[0029] Step 2, preparing a transition glaze layer, the mass ratio of each component of the transition glaze layer is: 20 parts of cobalt oxide powder, 60 parts of silicon dioxide powder, 20 parts of low-temperature frit powder, and 60 parts of water;
[0030] Step 3, uniformly mix the components described in step 2, stir for 30 minutes, and let stand for 10 minutes;
[0031] Step 4, erect the iron plate vertically, and spray the transition glaze layer prepared in step 3 onto the surface of the iron plate with a spray gun;
[0032] Step 5: Preliminary firing of the iron plate sprayed with the transition glaze layer by means of ceramic vertical kiln hanging firing, the firing temperature is 800 ° C, the firing time is 2 hours, and cooli...
Embodiment 2
[0040] A method for making an iron plate enamel decorative painting, comprising the following steps:
[0041] Step 1, select the iron plate, and use a sandblasting and dust removal machine to sandblast and derust the surface of the iron plate;
[0042] Step 2, preparing a transition glaze layer, the mass ratio of each component of the transition glaze layer is: 25 parts of cobalt oxide powder, 70 parts of silicon dioxide powder, 250 parts of low-temperature frit powder, and 65 parts of water;
[0043] Step 3, uniformly mix the components described in step 2, stir for 45 minutes, and let stand for 20 minutes;
[0044] Step 4, erect the iron plate vertically, and spray the transition glaze layer prepared in step 3 onto the surface of the iron plate with a spray gun;
[0045] Step 5: Preliminarily fire the iron plate coated with the transition glaze layer by hanging firing in a ceramic vertical kiln, the firing temperature is 850°C, the firing time is 2.5 hours, and then cool do...
Embodiment 3
[0053] A method for making an iron plate enamel decorative painting, comprising the following steps:
[0054] Step 1, select the iron plate, and use a sandblasting and dust removal machine to sandblast and derust the surface of the iron plate;
[0055] Step 2, preparing a transition glaze layer, the mass ratio of each component of the transition glaze layer is: 30 parts of cobalt oxide powder, 80 parts of silicon dioxide powder, 30 parts of low-temperature frit powder, and 70 parts of water;
[0056] Step 3, uniformly mix the components described in step 2, stir for 60 minutes, and let stand for 30 minutes;
[0057] Step 4, erect the iron plate vertically, and spray the transition glaze layer prepared in step 3 onto the surface of the iron plate with a spray gun;
[0058] Step 5: Preliminary firing of the iron plate sprayed with the transition glaze layer is carried out by using the ceramic vertical kiln hanging firing method, the firing temperature is 900 ° C, the firing tim...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com