A production method and density board technology, which is applied in the field of production of thin and environmentally friendly density boards for children's puzzles, can solve the problems of children's health threats, high formaldehyde content, poor water resistance, etc., and achieve improved waterproof performance, low formaldehyde release, and improved mechanical properties Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A method for producing thin environmentally-friendly density boards for children's jigsaw puzzles, comprising the following steps:
[0019] (1) Slicing poplar branches into wood chips of 60×30×5mm, and then cooking the chips with cooking liquid, the cooking temperature is 175°C, and the cooking time for maintaining this temperature is 35 minutes, wherein the cooking liquid is made of Made from the following components in parts by weight: 29 parts of False Betel, 18 parts of Nasturtium, 11 parts of Linden Flower, 8 parts of Albizia Julibrissin, 5 parts of Inula, 2 parts of Gourilla, and 860 parts of water;
[0020] (2) Thermally grind the cooked wood chips into fibers, then add 5% of its weight additives to the fibers, mix and stir evenly to obtain wet fibers, wherein the additives are made of the following components by weight: lignosulfonic acid 3 parts of sodium, 15 parts of cellulose acetate succinate;
[0021] (3) Apply the adhesive to the wet fiber delivery pipeli...
Embodiment 2
[0028] A method for producing thin environmentally-friendly density boards for children's jigsaw puzzles, comprising the following steps:
[0029] (1) Slicing poplar branches into wood chips of 60×30×5mm, and then cooking the chips with cooking liquid, the cooking temperature is 178°C, and the cooking time for maintaining this temperature is 38 minutes, wherein the cooking liquid is made of Made from the following components in parts by weight: 31 parts of betel, 20 parts of nasturtium, 13 parts of linden flower, 10 parts of albizia julibrissin, 7 parts of inula inula, 3 parts of gourami, and 880 parts of water;
[0030] (2) Thermally grind the cooked wood chips into fibers, then add 7% of its weight additives to the fibers, mix and stir evenly to obtain wet fibers, wherein the additives are made of the following components by weight: lignosulfonic acid Sodium 5 parts, cellulose acetate succinate 18 parts;
[0031] (3) Apply the adhesive to the wet fiber delivery pipeline thr...
Embodiment 3
[0038] A method for producing thin environmentally-friendly density boards for children's jigsaw puzzles, comprising the following steps:
[0039] (1) Slicing poplar branches into wood chips of 60×30×5mm, and then cooking the chips with cooking liquid at a temperature of 180°C, and the cooking time for maintaining this temperature is 40 minutes, wherein the cooking liquid is made of Made from the following components in parts by weight: 33 parts of betel, 22 parts of nasturtium, 15 parts of linden flower, 12 parts of albizia juliensis, 9 parts of inula inula, 4 parts of mulberry, and 900 parts of water;
[0040] (2) Thermally grind the cooked wood chips into fibers, then add 8% of its weight additives to the fibers, mix and stir evenly to obtain wet fibers, wherein the additives are made of the following components by weight: lignosulfonic acid Sodium 6 parts, cellulose acetate succinate 20 parts;
[0041] (3) Apply the adhesive to the wet fiber delivery pipeline through the ...