Method for removing impurities in reduced gold powder
A technology for reducing gold powder and impurities, which is applied in the field of removing impurities in reduced gold powder, can solve the problems of high impurity content, affecting product quality, etc., achieve good effect of removing impurities, ensure the quality of gold ingots, and shorten the processing time
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] 1) Add 3~5mol / L hydrochloric acid solution into the reaction kettle according to the liquid-solid ratio of 4:1, start stirring, adjust the rotation speed to 150r / min, feed steam to heat, and slowly raise the temperature to 60~80°C; The total amount of hydrochloric acid solution is 600L.
[0022] 2) Weigh 150kg of reduced gold powder and add it to the reaction kettle. The Ag content of the reduced gold powder is 0.0065%, the Cu content is 0.0038%, and the content of other miscellaneous items does not exceed the standard. Deposition at the bottom of the kettle;
[0023] 3) Weigh sodium chlorate according to 3% of the weight of the gold powder and dissolve it in water to make a solution for use. After step 2) the gold powder is added, add the sodium chlorate solution at one time, react for 2 to 3 hours, and then discharge and filter; chloric acid The solute mass fraction of the sodium solution was 25%.
[0024] 4) Wash the gold powder obtained in step 3) with hot water a...
Embodiment 2
[0028] 1) Add 3~5mol / L hydrochloric acid solution into the reaction kettle according to the liquid-solid ratio of 4:1, start stirring, adjust the rotation speed to 150r / min, feed steam to heat, and slowly raise the temperature to 60~80°C; The total amount of hydrochloric acid solution is 500L.
[0029] 2) Weigh 125kg of reduced gold powder and add it to the reaction kettle. The Pb content of the reduced gold powder is 0.0028%, and the content of other miscellaneous items does not exceed the standard. The feeding speed of gold powder does not exceed 5g / L per minute to prevent gold powder from depositing at the bottom of the reaction kettle;
[0030] 3) Weigh sodium chlorate according to 2.5% of the weight of the gold powder and dissolve it in water to prepare a solution for use. After the gold powder is added in step 2), add the sodium chlorate solution at one time, react for 2~3 hours, and then discharge and filter; chloric acid The solute mass fraction of the sodium solution ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com