Textured multicolor paint and preparation method thereof
A technology of colorful paint and texture, applied in the field of paint, can solve problems such as uneven effect, uneven spraying, and paint surface blooming, etc., and achieve the effect of enhancing the toughness of color dots
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2019-12-31
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 1 
Figure 2 
Figure 3
Abstract
Description
Technical field
[0001] The invention relates to the technical field of coatings, in particular to a textured colorful coating and a preparation method thereof. Background technique
[0002] Real stone paint is a kind of paint whose decorative effect resembles marble and granite. It is mainly made of natural stone powder of various colors and is applied to the imitation stone effect of building exterior walls, so it is also called liquid stone. Buildings decorated with real stone lacquer have natural and natural colors, giving people an elegant, harmonious and solemn beauty, and are suitable for indoor and outdoor decoration of various buildings. Especially the decoration on curved buildings is vivid and lifelike, and has a return to nature effect. However, the core raw material, natural colored sand, has serious color difference, which affects the visual sensory effect of real stone paint. Real stone paint needs to be matched with different colored sand to imitate the stone eff...
Examples
Embodiment 1
[0060] A kind of colorful texture paint, in parts by mass, the components are as follows:
[0061] Protective glue:
[0062]
[0063] Toning base material:
[0064]
[0065]
[0066] Texture paint precursor
[0067]
[0068]
[0069] Continuous phase:
[0070]
[0071] Preparation:
[0072] (1) Preparation of protective glue for use: Add deionized water to the container and stir at a stirring speed of 300-600r / min. Add dispersant, viscosity reducer, antifungal agent, fungicide, pH regulator, and stir for 1 -2min; Adjust the stirring speed to 1300-1500r / min, add protective rubber powder and stir for 50min to prepare a protective glue slurry;
[0073] (2) Prepare the tinting base material for future use:
[0074] a. Add deionized water to the container and stir;
[0075] b. Under stirring at 300-500rpm, add mildew inhibitor and dispersant evenly and slowly and stir for 1-2min;
[0076] c. Under 600-800rpm stirring, add cellulose and stir for 5-10min;
[0077] d. Under 700-900rpm stirring, slow...
Embodiment 2
[0101] A kind of colorful texture paint, in parts by mass, the components are as follows:
[0102] Protective glue:
[0103]
[0104]
[0105] Toning base material:
[0106]
[0107]
[0108] Texture paint precursor:
[0109]
[0110] Continuous phase:
[0111]
[0112]
[0113] Preparation:
[0114] (1) Preparation of protective glue for use: Add deionized water to the container and stir at a stirring speed of 300-600r / min. Add dispersant, viscosity reducer, antifungal agent, fungicide, pH regulator, and stir for 1 -2min; Adjust the stirring speed to 1300-1500r / min, add protective rubber powder and stir for 50min to prepare a protective glue slurry;
[0115] (2) Prepare the tinting base material for future use:
[0116] a. Add deionized water to the container and stir;
[0117] b. Under stirring at 300-500rpm, add mildew inhibitor and dispersant evenly and slowly and stir for 1-2min;
[0118] c. Under 600-800rpm stirring, add cellulose and stir for 5-10min;
[0119] d. Under 700-900rpm stir...
Embodiment 3
[0143] A kind of colorful texture paint, in parts by mass, the components are as follows:
[0144] Protective glue:
[0145]
[0146] Toning base material:
[0147]
[0148]
[0149] Texture paint precursor:
[0150]
[0151] Continuous phase:
[0152]
[0153] Preparation:
[0154] (1) Preparation of protective glue for use: Add deionized water to the container and stir at a stirring speed of 300-600r / min. Add dispersant, viscosity reducer, antifungal agent, fungicide, pH regulator, and stir for 1 -2min; Adjust the stirring speed to 1300-1500r / min, add protective rubber powder and stir for 50min to prepare a protective glue slurry;
[0155] (2) Prepare the tinting base material for future use:
[0156] a. Add deionized water to the container and stir;
[0157] b. Under stirring at 300-500rpm, add mildew inhibitor and dispersant evenly and slowly and stir for 1-2min;
[0158] c. Under 600-800rpm stirring, add cellulose and stir for 5-10min;
[0159] d. Under 700-900rpm stirring, slowly add f...