[0026] An alloy copper remover for a gun is composed as follows in parts by weight: 25% of bismuth; 50% of lead; 25% of indium.
[0027] A preparation method of alloy copper remover for guns, comprising the following steps:
[0028] Step 1, heat the prepared lead, indium, and bismuth metals with a purity of more than 99.99% to 450°C, stir and mix them thoroughly, and then keep them warm for 30 minutes;
[0029] Step 2, after natural cooling, repeat heating three times, all heated to 450°C, then fully stirred, keep warm for 30 minutes and cool naturally to ensure that the metals are fully mixed to obtain a metal alloy block;
[0030] Step 3, the cooled metal alloy block is made into powder by rotating electrode atomization method under the conditions of electrode rod speed of 12000r / min, current intensity of 1500A, and feed rate of 1.0mm / s, which is to remove copper from the alloy agent.
[0031] The contact angle between 25In-50Pb-Bi and copper plate is 24°, and it has excel...
Embodiment 2
[0033] An alloy copper remover for a gun is composed as follows in parts by weight: 27% of bismuth; 56% of lead; and 17% of indium.
[0034] A preparation method of alloy copper remover for guns, comprising the following steps:
[0035] Step 1, heat the prepared lead, indium, and bismuth metals with a purity of more than 99.99% to 450°C, stir and mix them thoroughly, and then keep them warm for 30 minutes;
[0036] Step 2, after natural cooling, repeat heating three times, all heated to 450°C, then fully stirred, keep warm for 30 minutes and cool naturally to ensure that the metals are fully mixed to obtain a metal alloy block;
[0037] Step 3, the cooled metal alloy block is made into powder by rotating electrode atomization method under the conditions of electrode rod speed of 12000r / min, current intensity of 1500A, and feed rate of 1.0mm / s, which is to remove copper from the alloy agent.
[0038] In this embodiment, the contact angle between 17In-56Pb-Bi and the copper pl...
Embodiment 3
[0040] An alloy copper remover for a gun is composed as follows in parts by weight: 25% of bismuth; 60% of lead; and 15% of indium.
[0041] A preparation method of alloy copper remover for guns, comprising the following steps:
[0042] Step 1, heat the prepared lead, indium, and bismuth metals with a purity of more than 99.99% to 450°C, stir and mix them thoroughly, and then keep them warm for 30 minutes;
[0043]Step 2, after natural cooling, repeat heating three times, all heated to 450°C, then fully stirred, keep warm for 30 minutes and cool naturally to ensure that the metals are fully mixed to obtain a metal alloy block;
[0044] Step 3, the cooled metal alloy block is made into powder by rotating electrode atomization method under the conditions of electrode rod speed of 12000r / min, current intensity of 1500A, and feed rate of 1.0mm / s, which is to remove copper from the alloy agent.
[0045] In this embodiment, the contact angle between 15In-60Pb-Bi and the copper pla...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com