A chemical fiber and functional technology, which can be applied in the field of increasing the water absorption and moisture removal function of chemical fiber, can solve the problem that the water absorption and moisture removal function cannot surpass natural fibers and other problems, and achieve the effect of breaking through the technical bottleneck.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0026] A 100D polyester filament that can increase the function of water absorption and moisture release.
[0027] In the first step, the 100D polyester filament is added to 26T / cm on the basis of 16T / cm according to the technical requirements of the customer, and the twist is S twist.
[0028] In the second step, the hydrolyzable polyester yarn 50D and the twisted 100D, 26T / cm, S twisted polyester yarn are twisted in the Z direction to add 10T / cm, and the Z direction is stranded.
[0029] In the third step, twisting 100D polyester filaments and strands twisted with 50D hydrolyzable polyester filaments is subjected to high-temperature and high-pressure shaping at a temperature of 120° C. for half an hour.
[0030] In the fourth step, the hydrolyzable polyester filaments in the strands are hydrolyzed.
[0031] Use 5g / L of 98% caustic soda, 0.4g / L of silk-removing agent DYT, and 0.5g / L of acetic acid to form a solution with a ratio of 1:15.
[0032] Put the strands into the aq...
Embodiment 2
[0035] A polyester taffeta with increased moisture wicking properties.
[0036] The first step is to add 50D polyester filament S twist to 28T / cm on the basis of 18T / cm and S twist according to customer requirements.
[0037] In the second step, the 45D hydrolyzable polyester filament and the twisted 50D, 28T / cm, S-twisted polyester filament are twisted 10T / cm in the Z direction and formed into strands.
[0038] In the third step, the strands are subjected to high temperature and high pressure setting at a temperature of 120° C. for 45 minutes.
[0039] The fourth step is to weave the strands into cloth according to the technical requirements of polyester taffeta.
[0040] The fifth step is to hydrolyze the hydrolyzable polyester filaments in the woven gray cloth.
[0041] Use 2g / L of non-ionic hydrogen peroxide stabilizer, 6g / L of hydrogen peroxide with a concentration of 27.5%, 6g / L of caustic soda with a concentration of 98%, 0.4g / L of silk-removing agent DYT, and 0.1g / L ...