[0015] A kind of preparation method of 3D art floor of the present invention comprises the following steps:
[0016] Step 1. Mix the primer and curing agent evenly according to the mass ratio of 2:1, then divide them into two parts, add different color pastes respectively, and obtain component A and component B;
[0017] Step 2. Use component A as a pavement on the ground to form a floor primer, then spray component B on the floor primer, and naturally cure to obtain a 3D art floor;
[0018] In parts by weight, the primer includes 800-1000 parts of epoxy resin dispersion, 50-100 parts of dipropylene glycol butyl ether, 1-10 parts of wetting agent, 1-10 parts of defoamer, 50-100 parts of 5% RD sol, 10-100 parts of thickener and 5-50 parts of pearlescent filler;
[0019] The curing agent is an epoxy resin curing agent.
[0020] It can be seen from the above description that the beneficial effect of the present invention lies in: the preparation method of the 3D art floor provi...
Embodiment 1
[0030] The preparation method of 3D art floor, comprises the following steps:
[0031] Step 1. Mix the primer and curing agent evenly according to the mass ratio of 2:1, then divide them into two parts, add different color pastes respectively, and get A component (white) and B component (blue);
[0032] Step 2. Spread component A on the ground to form a floor primer, and then spray component B on the floor primer. After natural curing, a 3D artistic floor is obtained. See figure 1 shown;
[0033] In parts by weight, the primer includes 800kg of 0901 epoxy resin dispersion, 50kg of DPn, 1kg of SURFYNOL 104E wetting agent, 3kg of RHODOLINE DF691 defoamer, 50kg of 5% RD sol, 30kg of U905 thickener and 20kg of KC8100 color pearlescent pigment;
[0034] The 5% RD sol is composed of 5% RD rubber powder, 0.1% LEX preservative and the balance water, and the RD rubber powder is LAPONITE RD;
[0035] The curing agent is 332 curing agent.
Embodiment 2
[0037] The preparation method of 3D art floor, comprises the following steps:
[0038] Step 1. Mix the primer and curing agent evenly according to the mass ratio of 2:1, then divide them into two equal parts, and add white and blue colorants respectively to obtain component A (white) and component B (black);
[0039] Step 2. Spread component A on the ground to form a floor primer, and then spray component B on the floor primer. After natural curing, a 3D artistic floor is obtained. See figure 2 shown;
[0040] In parts by weight, the primer includes 900kg of 0901 epoxy resin dispersion, 80kg of DPn, 5kg of SURFYNOL 104E wetting agent, 1kg of RHODOLINE DF691 defoamer, 70kg of 5% RD sol, 10kg of U905 thickener and 5kg of KC8100 color pearlescent pigment;
[0041] The 5% RD sol is composed of 5% RD rubber powder, 0.1% LEX preservative and the balance water, and the RD rubber powder is LAPONITE RD;
[0042] The curing agent is 332 curing agent.