Embodiment 1
[0020] A method for preparing an environment-friendly fabric coating for travel luggage, prepared from the following raw materials in parts by mass: 60 parts of polymer diol, 30 parts of diisocyanate, 1 part of catalyst, 1 part of plasticizer, and neutralizer 3 parts, 120 parts of deionized water, 10 parts of nano silicon dioxide, 8 parts of epoxy soybean oil, 10 parts of acetone, 2 parts of crosslinking agent.
[0021] The manufacturing method of this embodiment includes the following steps:
[0022] Step 1: Add polymer diol, diisocyanate, catalyst, and plasticizer into the mixer, set the rotation speed to 1000r / min, set the temperature to 120°C, and set the time to 60min to obtain a mixture;
[0023] Step 2: Add the neutralizer and half of the deionized water into the mixture, set the rotation speed to 200r / min, the temperature to 20°C, and the time to 30min to prepare a water-based polyurethane emulsion;
[0024] Step 3: Add epoxy soybean oil, acetone, cross-linking agent ...
Embodiment 2
[0026] A method for preparing an environment-friendly fabric coating for travel luggage, prepared from the following raw materials in parts by mass: 65 parts of polymer diol, 35 parts of diisocyanate, 1 part of catalyst, 1 part of plasticizer, and neutralizer 4 parts, 130 parts of deionized water, 12 parts of nano silicon dioxide, 10 parts of epoxidized soybean oil, 11 parts of acetone, 3 parts of crosslinking agent.
[0027] The manufacturing method of this embodiment includes the following steps:
[0028] Step 1: Add polymer diol, diisocyanate, catalyst, and plasticizer into the mixer, set the rotation speed to 1000r / min, set the temperature to 120°C, and set the time to 60min to obtain a mixture;
[0029] Step 2: Add the neutralizer and half of the deionized water into the mixture, set the rotation speed to 200r / min, the temperature to 20°C, and the time to 30min to prepare a water-based polyurethane emulsion;
[0030] Step 3: Add epoxy soybean oil, acetone, cross-linking ...
Embodiment 3
[0033] A method for preparing an environment-friendly fabric coating for travel luggage, prepared from the following raw materials in parts by mass: 70 parts of polymer diol, 40 parts of diisocyanate, 1 part of catalyst, 2 parts of plasticizer, and neutralizer 4 parts, 140 parts of deionized water, 15 parts of nano silicon dioxide, 12 parts of epoxy soybean oil, 13 parts of acetone, 5 parts of crosslinking agent.
[0034] The manufacturing method of this embodiment includes the following steps:
[0035] Step 1: Add polymer diol, diisocyanate, catalyst, and plasticizer into the mixer, set the rotation speed to 1200r / min, set the temperature to 180°C, and set the time to 60min to obtain a mixture;
[0036] Step 2: Add the neutralizer and half of the deionized water into the mixture, set the rotation speed to 300r / min, the temperature to 40°C, and the time to 60min to prepare a water-based polyurethane emulsion;
[0037] Step 3: Add epoxy soybean oil, acetone, cross-linking agen...