Multiple-effect solid inhibiting anti-scale rod
A technology of corrosion and scale inhibition and corrosion and scale inhibitors, which is applied in wellbore/well components, earthwork drilling and production, etc., which can solve the problems of shortened equipment life, high flow rate, and liquid corrosion inhibitors are easily taken out quickly.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0023] The multi-effect perimeter antiscaling rod components are composed of the following components in weight percent: polyvinyl alcohol 8%; polymaleic anhydride and hydroxyethylene diphosphonic acid 15%; zinc chloride 30%; epoxy resin 10%; Alkyl dimethyl benzyl ammonium chloride 2%; water 35%.
[0024] The preparation process of the composition of the present invention is as follows: according to the formula of the above-mentioned composition weight percentage, mix the 1:1 mixture of raw material polymaleic anhydride and hydroxyethylene diphosphonic acid with zinc chloride, add the above-mentioned formula Water in percentage by weight, then slowly add polyvinyl alcohol, stir, and knead in a kneader for 5 hours at 80°C. During the kneading process, add 1% of the catalyst ammonium persulfate in the total amount of the above composition. When the kneaded mixture is close to dryness, add Dodecyl dimethyl benzyl ammonium chloride, the reactant is quickly dried and crushed, and e...
example 1
[0025] The linear polarization corrosion rate and pitting coefficient of the corrosion and scale inhibition rod described in Example 1 were continuously monitored for 10 days as shown in FIG. 1 .
[0026] It can be seen from the test results that with the prolongation of the monitoring time, the linear polarization corrosion rate sum (LPR) and the pitting coefficient (PF) gradually decrease and tend to be stable, showing good corrosion inhibition performance. The scale inhibition rate reaches 79%.
[0027] Through continuous monitoring for 10 days, it can be seen that the change trend of linear polarization corrosion rate (LPR) is shown in Figure 1.
[0028] It can be seen from Figure 1 that: with the extension of time and the continuous release of active ingredients, the linear corrosion rate (LPR) is controlled below the standard of less than 0.076mm / y. The pitting coefficient (PF) is within the safe limit (less than 0.1)
[0029] The field test of four wells has been carr...
Embodiment 2
[0032] The multi-effect solid antiscaling rod component is composed of the following components in weight percentage: polyacrylamide 10%; polymaleic anhydride and hydroxyethylene diphosphonic acid 20%; zinc oxide 35%; calcium stearate 10%; Dialkyl dimethyl benzyl ammonium chloride 5%; water 20%.
[0033] The preparation process and parameters of this example are the same as those in Example 1, and the difference compared with Example 1 is that in the preparation process, polyacrylamide is used as the polymer forming agent instead of polyvinyl alcohol, and zinc oxide is used as the synergist instead of zinc chloride. Binding agent has replaced epoxy resin with calcium stearate, and present embodiment technological process and process parameter are as follows:
[0034] Prepared according to the weight percent formula of the above composition, mix the 1:1 mixture of raw material polymaleic anhydride and hydroxyethylene diphosphonic acid with zinc oxide evenly, add the water of th...
PUM
Login to View More Abstract
Description
Claims