Non-toxic environment protective solvent type bridge floor water-proofing material and preparation thereof
A waterproof material, non-toxic and environmentally friendly technology, applied in building insulation materials, chemical instruments and methods, other chemical processes, etc., can solve problems such as easy to be punctured, not widely used, tight fit, etc., and achieve excellent high and low temperature performance , high bonding strength, good waterproof performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] (1) Weigh the raw materials according to the following proportions
[0019] Base Asphalt Korea SK70# 100kg
[0020] Synthetic rubber styrene-butadiene-styrene block polymer SBS792 10kg
[0021] Organic solvent cyclohexane 120kg
[0022] Tackifier Terpene Resin 20kg
[0023] Light Stabilizer Phenyl Salicylate 3kg
[0024] Plasticizer dimethyl phthalate 2kg
[0025] Preparation Process
[0026] Step 1: Place the organic non-toxic solvent cyclohexane in the reactor, start stirring, then add rubber modifier SBS, tackifier terpene resin T110 and plasticizer dimethyl phthalate in sequence, cover Lid, stirring at a constant speed of 50-100r / min for 10-30 minutes;
[0027] Step 2: Open the reaction kettle, then add 70# or 90# hot asphalt and light stabilizer phenyl salicylate in sequence at 140~170℃, close the lid, continue stirring at 50~100r / min speed for 15~30 minutes, naturally cool down;
[0028] Step 3: When the temperature drops below 30°C, the reaction kettle is...
Embodiment 2
[0033] (2) Weigh the raw materials according to the following proportions
[0034] Base Asphalt Korea SK70# 100kg
[0035] Synthetic rubber styrene-butadiene-styrene block polymer SBS792 20kg
[0036] Organic solvent cyclohexane 160kg
[0037] Tackifier Terpene Resin 60kg
[0038] Light Stabilizer Phenyl Salicylate 5kg
[0039] Plasticizer dimethyl phthalate 6kg
[0040] Preparation Process
[0041] The preparation process is the same as in Example 1
[0042] The performance of the modified emulsified asphalt waterproof material and the non-toxic and environmentally friendly solvent-based bridge deck waterproof material was compared by the method of the comparative test. The test results are listed in Table 2.
[0043] Table 2 Performance comparison of modified emulsified asphalt waterproof material and non-toxic and environmentally friendly solvent-based bridge deck waterproof material
[0044] Test items
Embodiment 3
[0046] (3) Weigh the raw materials according to the following proportions
[0047] Base Asphalt Korea SK70# 100kg
[0048] Synthetic rubber styrene-butadiene-styrene block polymer SBS792 30kg
[0049] Organic solvent cyclohexane 200kg
[0050] Tackifier Terpene Resin 100kg
[0051] Light Stabilizer Phenyl Salicylate 7kg
[0052]Plasticizer dimethyl phthalate 10kg
[0053] Preparation Process
[0054] The preparation process is the same as in Example 1.
[0055] The performance of the modified emulsified asphalt waterproof material and the non-toxic and environmentally friendly solvent-based bridge deck waterproof material was compared by the method of the comparative test. The test results are listed in Table 3.
[0056] Table 3 Performance comparison of modified emulsified asphalt waterproof material and non-toxic and environmentally friendly solvent-based bridge deck waterproof material
[0057] Test items
Technical indicators
Modifi...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com