preparation example 1
[0112] Take the following weight materials to prepare functional emulsion:
[0113] Microcapsule phase change material (PCM): 200g,
[0114] Nano ZnO: 10% by weight of PCM,
[0115] Water: add up to 1000ml.
[0116] The microcapsule phase change material was purchased from Hong Kong Nano Sports Tech. Company, the model is TRC-05-01, and the phase change temperature of the phase change material is 28°C. Wherein the microcapsule phase change material is the weight of solid matter. Add PCM to an appropriate amount of water, add ZnO (MN6Z, Zhejiang Hongsheng Material Technology Co., Ltd.) under slow stirring, and stir at room temperature for 2.5 hours to obtain the functional emulsion of the present invention.
preparation example 2
[0118] Take the following weight materials to prepare functional emulsion:
[0119] Microcapsule phase change material (PCM): 400g,
[0120] Nano ZnO: 0.5% by weight of PCM,
[0121] Adhesive LT 200g
[0122] Water: add up to 1000ml.
[0123] The microcapsule phase change material was purchased from Hong Kong Nano Sports Tech. Company, the model is TRC-05-01, and the phase change temperature of the phase change material is 28°C. Wherein the microcapsule phase change material is the weight of solid matter. Add PCM to an appropriate amount of water, add ZnO under slow stirring, and stir at room temperature for 2.5 hours to obtain the functional emulsion of the present invention.
preparation example 3
[0125] Take the following weight materials to prepare functional emulsion:
[0126] Microencapsulated phase change material (PCM): 5g,
[0127] Nano-TiO 2: 30% of PCM weight,
[0128] KC softener (produced by Shanghai Auxiliary Factory) 25g,
[0129] Synthetic styrene-butadiene emulsion 180g,
[0130] Water: add up to 1000ml.
[0131] Among them, the microcapsule phase change material was purchased from Hong Kong Nano Sports Tech. Company, the model is TRC-05-01A. Wherein the microcapsule phase change material is the weight of solid matter. Add PCM to an appropriate amount of water, and add nano-TiO while stirring slowly 2 (SCI-nanometer titanium dioxide, Shanghai Zhuerna High-tech Powder Material Co., Ltd.), stirred at room temperature for 2.5 hours to obtain the functional emulsion of the present invention.
PUM
Property | Measurement | Unit |
---|---|---|
Phase transition temperature | aaaaa | aaaaa |
Particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com